Abstract

This document gives specific procedures for industrial X-ray and gamma radiography for discontinuity detection purposes, using NDT (non-destructive testing) film techniques. This part of the EN 12681 series specifies the requirements for film radiographic testing of castings.
Films after exposure and processing become radiographs with different area of optical density. Radiographs are viewed and evaluated using industrial radiographic illuminators.
This part of the EN 12681 series specifies the recommended procedure for the choice of operating conditions and radiographic practice.
These procedures are applicable to castings produced by any casting process, especially for steel, cast iron, aluminium, cobalt, copper, magnesium, nickel, titanium, zinc and any alloys of them.
NOTE   This document considers EN ISO 5579.
This document does not apply to:
-   radiographic testing of castings for aerospace applications (see EN 2002-21);
-   radiographic testing of welded joints (see EN ISO 17636-1);
-   radiography with digital detectors (see EN 12681-2);
-   radioscopic testing (see the EN 13068 series).

Status
Published
Publication Date
10-Nov-2026
Current Stage
6060 - Definitive text made available (DAV) - Publishing
Start Date
11-Nov-2026
Due Date
27-Jul-2027
Completion Date
27-Jul-2027

Buy Documents

Standard

EN 12681-1:2027

English language (51 pages)
Preview
Preview
e-Library read for
×1 day

EN 12681-1:2026 is a CEN standard for industrial X-ray and gamma radiography of castings using film techniques. It specifies how to choose the radiographic setup, film system, image quality and acceptance criteria for detecting internal discontinuities, mainly for foundries and for the people who specify, perform or evaluate casting radiography.

What does EN 12681-1:2026 specify?

EN 12681-1:2026 specifies film radiographic testing for castings produced by any casting process, with particular application to steel, cast iron, aluminium, cobalt, copper, magnesium, nickel, titanium, zinc and their alloys. It covers how to plan the exposure, how to view the radiograph and how to judge acceptability.

The document is built around Clauses 1 to 19 and Annexes A to H. It uses EN ISO 5579 as its basic radiographic framework and then adds casting-specific procedures, image quality values and severity levels.

AnnexWhat it covers
Annex AMinimum image quality values
Annex BSeverity levels for steel castings
Annex CSeverity levels for cast iron castings
Annex DSeverity levels for aluminium alloy and magnesium alloy castings
Annex ESeverity levels for copper alloy castings
Annex FSeverity levels for titanium and titanium alloy castings
Annex GSignificant technical changes from the previous edition
Annex HCalculation of maximum X-ray tube voltages in Figure 13

EN 12681-1:2026 does not apply to aerospace castings, welded joints, radiography with digital detectors, or radioscopic testing.

What are the key requirements of EN 12681-1:2026?

EN 12681-1:2026 is organized around a few practical decisions: which testing class to use, how to set up the exposure, which film system and source to use, how to verify image quality, and how to judge the result. Those decisions determine whether a radiograph can reliably show discontinuities in a casting.

Choosing the test conditions

Clause 5 divides radiographic techniques into testing class A and testing class B. Class A is the basic option, and class B is used when class A is not sensitive enough. If a class B condition cannot be met for technical or industrial reasons, the parties may agree to use the class A condition, but the loss of sensitivity has to be compensated by higher minimum optical density or by a film system two classes better.

Clause 6 requires suitable surface preparation, unless the surface condition is already adequate, and radiography is normally carried out after the final manufacturing stage. It also requires the areas that cannot be tested, or can only be partly tested, to be identified in advance and shown on the film position plan. Personnel are to be qualified in accordance with EN ISO 9712 or equivalent.

Setting up the exposure

Clause 7 sets the permitted test arrangements for single-wall, double-wall and complex geometries, using Figures 1 to 12. Clause 8 says the X-ray tube voltage should be as low as possible for good sensitivity, while still matching the penetrated thickness and material. Clause 8 also gives the thickness ranges for gamma sources and higher-energy X-ray equipment, and it notes that gamma sources are used when X-ray tubes are difficult to apply.

Clause 9 ties the film system class and metal screens to the radiation source and thickness range. This matters because film speed, screen choice and contact between film and screens directly affect sensitivity and image quality. Clauses 10 and 11 then address scatter and geometry: collimation, backscatter checks, and minimum source-to-object distance are all used to keep image unsharpness and unwanted radiation low.

Making the radiograph readable

Clause 12 sets minimum optical density values for the evaluated area, with a higher value for testing class B than for class A. It also limits fog density and requires the viewer to be able to show the maximum readable optical density. Clause 13 requires controlled film processing and darkroom viewing on an adjustable-luminance viewer in a masked viewing area.

Clause 14 allows methods for covering a larger thickness range in one exposure, including multiple film techniques, higher radiation energy, beam hardening and thickness equalization. Clause 15 requires clear identification of the radiograph and test area, marking or recording of the test area location, and sufficient overlap when several films are used. These requirements matter in practice because they prevent wrong-location readings and missed coverage.

Verifying quality and deciding acceptance

Clause 16 requires image quality verification with an IQI, normally in accordance with EN ISO 19232-1 or EN ISO 19232-2. The IQI is normally placed on the source side, and the clause gives fallback arrangements when that is not possible. Annex A gives the minimum image quality values, and Table A.3 gives specific exceptions for some gamma-ray cases.

Clause 18 defines acceptance by severity levels and reference radiographs. Annexes B to F provide the material-specific severity levels for steel, cast iron, aluminium and magnesium, copper alloys, and titanium. Clause 18.3 also divides the wall section into rim zone and core zone, which matters because the acceptance limit can depend on where the discontinuity is found.

Clause 19 requires a test report for each exposure or set of exposures, with the testing body, casting identification, material, thickness, acceptance criteria, source details, film system, exposure conditions, IQI data, evaluation results and any agreed deviation.

What terms does EN 12681-1:2026 define?

  • Wall thickness - the thickness measured on the casting.
  • Nominal wall thickness - the thickness specified on the drawing.
  • Penetrated thickness (w) - the thickness of material in the beam direction, based on all penetrated walls.
  • Source size - the size of the radiation source or focal spot size.
  • Object-to-film distance (b) - the largest distance between the source side of the part and the film surface along the beam axis.
  • Source-to-object distance (f) - the distance from the radiation source to the source side of the test object along the beam axis.
  • Source-to-film distance (SFD) - the distance from the source to the film, equal to f + b.
  • Image quality indicator (IQI) - the indicator used to verify whether the radiograph meets the required image quality.

Who uses EN 12681-1:2026?

EN 12681-1:2026 is used by foundries, radiographic testing laboratories, NDT personnel, quality managers, buyers and contracting parties who need to agree how castings will be examined and accepted. It is relevant wherever castings are inspected for internal discontinuities such as gas holes, non-metallic inclusions, shrinkage, cracks and inserts.

The standard is especially useful when radiography has to be specified in an order, when a test arrangement must be selected for a difficult geometry, or when a radiograph has to be judged against agreed acceptance criteria.

What changed in EN 12681-1:2026 from the previous edition?

EN 12681-1:2026 is intended to supersede EN 12681-1:2017. The stated technical changes include:

  • ASTM reference radiograph standards were updated.
  • The term “class” was replaced by “testing class” for clarity.
  • Clause 7 was revised and missing figure captions were added.
  • Clause 8 was revised, including changes to the Se 75 thickness range and a note to Annex H.
  • Clause 11 was revised, with EN IEC 62976 added for LINAC focal spots and the nomogram corrected.
  • Annexes B to F were updated to the latest ASTM revisions.
  • Annex H was added.

Which standards are used with EN 12681-1:2026?

EN 12681-1:2026 relies on several companion standards:

  • EN ISO 5579 - basic rules for radiographic testing of metallic materials using film and X- or gamma rays.
  • EN ISO 5580 - minimum requirements for industrial radiographic illuminators.
  • EN ISO 9712 - qualification and certification of NDT personnel.
  • EN ISO 11699-1 - classification of industrial radiographic film systems.
  • EN ISO 11699-2 - control of film processing by reference values.
  • EN ISO 19232-1 and EN ISO 19232-2 - image quality indicators for wire and step/hole methods.
  • ISO 5576 - vocabulary for industrial X-ray and gamma-ray radiology.
  • Related parts named in the document include EN 12681-2 for digital detectors, EN 2002-21 for aerospace castings, and EN ISO 17636-1 for welded joints.

What does the EN 12681-1:2026 document contain?

EN 12681-1:2026 contains procedures, figures, tables and annexes that support daily radiographic practice rather than just a short rule set. The core clauses cover test arrangements, source selection, film systems, scatter reduction, exposure geometry, optical density, processing, viewing, image quality and acceptance.

It includes Figures 1 to 17 for test setups, geometry, tube voltage selection, thickness-range extension and wall-zone division. It also includes tables for optical density, film systems and screens, image quality requirements, and severity levels by material group.

The annexes provide the material-specific acceptance references and the minimum image quality values needed to use the standard in inspection, audit, and acceptance work.

Relations

Effective Date
02-Feb-2023
Effective Date
18-Nov-2026
Effective Date
18-Nov-2026
Effective Date
18-Nov-2026
Effective Date
18-Nov-2026
Effective Date
18-Nov-2026
Effective Date
18-Nov-2026
Effective Date
18-Nov-2026
Effective Date
18-Nov-2026
Effective Date
18-Nov-2026
Effective Date
18-Nov-2026
Effective Date
18-Nov-2026
Effective Date
18-Nov-2026
Effective Date
18-Nov-2026
Effective Date
18-Nov-2026

Buy Documents

Standard

EN 12681-1:2027

English language (51 pages)
Preview
Preview
e-Library read for
×1 day

Get Certified

Connect with accredited certification bodies for this standard

Element Materials Technology

Materials testing and product certification.

UKAS United Kingdom Verified

Inštitut za kovinske materiale in tehnologije

Institute of Metals and Technology. Materials testing, metallurgical analysis, NDT.

SA Slovenia Verified

Sponsored listings

Frequently Asked Questions

EN 12681-1:2026 is a standard published by the European Committee for Standardization (CEN). Its full title is "Founding - Radiographic testing - Part 1: Film techniques". This standard covers: This document gives specific procedures for industrial X-ray and gamma radiography for discontinuity detection purposes, using NDT (non-destructive testing) film techniques. This part of the EN 12681 series specifies the requirements for film radiographic testing of castings. Films after exposure and processing become radiographs with different area of optical density. Radiographs are viewed and evaluated using industrial radiographic illuminators. This part of the EN 12681 series specifies the recommended procedure for the choice of operating conditions and radiographic practice. These procedures are applicable to castings produced by any casting process, especially for steel, cast iron, aluminium, cobalt, copper, magnesium, nickel, titanium, zinc and any alloys of them. NOTE This document considers EN ISO 5579. This document does not apply to: - radiographic testing of castings for aerospace applications (see EN 2002-21); - radiographic testing of welded joints (see EN ISO 17636-1); - radiography with digital detectors (see EN 12681-2); - radioscopic testing (see the EN 13068 series).

This document gives specific procedures for industrial X-ray and gamma radiography for discontinuity detection purposes, using NDT (non-destructive testing) film techniques. This part of the EN 12681 series specifies the requirements for film radiographic testing of castings. Films after exposure and processing become radiographs with different area of optical density. Radiographs are viewed and evaluated using industrial radiographic illuminators. This part of the EN 12681 series specifies the recommended procedure for the choice of operating conditions and radiographic practice. These procedures are applicable to castings produced by any casting process, especially for steel, cast iron, aluminium, cobalt, copper, magnesium, nickel, titanium, zinc and any alloys of them. NOTE This document considers EN ISO 5579. This document does not apply to: - radiographic testing of castings for aerospace applications (see EN 2002-21); - radiographic testing of welded joints (see EN ISO 17636-1); - radiography with digital detectors (see EN 12681-2); - radioscopic testing (see the EN 13068 series).

EN 12681-1:2026 is classified under the following ICS (International Classification for Standards) categories: 77.040.20 - Non-destructive testing of metals. The ICS classification helps identify the subject area and facilitates finding related standards.

EN 12681-1:2026 has the following relationships with other standards: It is inter standard links to EN 12681-1:2017, EN 14141:2013, EN ISO 14096-2:2026, EN 14141:2003, EN 1559-4:1999, EN 12392:2016, EN 14096-2:2003, EN 1559-3:2011, EN ISO 14096-2:2020, EN 1559-2:2014, EN 13068-3:2001, EN 1559-6:1998, EN 13981-3:2006, EN 1559-5:1997, EN 1559-5:2017. Understanding these relationships helps ensure you are using the most current and applicable version of the standard.

EN 12681-1:2026 is available in PDF format for immediate download after purchase. The document can be added to your cart and obtained through the secure checkout process. Digital delivery ensures instant access to the complete standard document.

Standards Content (Sample)

Contents

  • Introduction
  • 1 Scope
  • 2 Normative references
  • 3 Terms and definitions
  • 3.1 wall thickness
  • 3.2 nominal wall thickness
  • 3.3 penetrated thickness
  • 3.4 source size
  • 3.5 object-to-film distance
  • 3.6 source-to-object distance
  • 3.7 source-to-film distance
  • 4 Symbols and abbreviated terms
  • 5 Classification of radiographic techniques
  • 6 General preparations and requirements
  • 6.1 General preparations
  • 6.2 Agreements
  • 6.3 Personnel qualification
  • 7 Test arrangements
  • 7.1 General
  • 7.2 Single wall penetration of plane areas
  • 7.3 Single wall penetration of curved areas
  • 7.4 Double wall penetration of plane and curved areas
  • 7.5 Choice of test arrangements for complex geometries
  • 7.6 Acceptable test area dimensions
  • 8 Choice of tube potential and radiation source
  • 8.1 X-ray devices up to 1 000 kV
  • 8.2 Other radiation sources
  • 9 Film systems and metal screens
  • 1 MV < X-ray 0,25 mm to 0,7 mm front and back screens
  • 4 MV < X-ray
  • 10 Reduction of scattered radiation
  • 10.1 Metal filters and collimators
  • 10.2 Interception of backscattered radiation
  • 11 Source-to-object distance
  • 12 Optical density D of radiograph
  • 13 Film processing and viewing
  • 13.1 Processing
  • 13.2 Film viewing conditions
  • 14 Techniques for increasing the covered thickness range
  • 14.1 General
  • 14.2 Multiple film technique
  • 14.3 Contrast decreasing by higher radiation energy
  • 14.4 Contrast decreasing by beam hardening
  • 14.5 Contrast decreasing by thickness equalization
  • 15 Requirements on radiographs
  • 15.1 Identification of radiograph, test area, film position plan
  • 15.2 Marking of the test areas
  • 15.3 Overlap of films
  • 16 Verification of image quality
  • 17 Influence of crystalline structure
  • 18 Acceptance criteria
  • 18.1 General
  • 18.2 Severity levels
  • 18.3 Wall section zones
  • 19 Test report
  • Annex A
  • Annex B
  • 3.2.5.1 positive
  • 3.2.5.2 Maximum allowable deviation shall
  • Annex C
  • Annex D
  • 3.2.4 round
  • 3.2.4 elongated
  • 3.2.10 sponge
  • 3.2.5 feathery
  • 3.2.6 sponge
  • 3.2.2 less dense
  • 3.2.2 more dense b
  • Annex E
  • Annex F
  • 5.1.2.3 cavity
  • Annex G
  • Annex H
  • Annex B to Annex F
  • Bibliography
  • Annex G “Calculation of maximum X-ray tube
  • Bibliography

Introduction

Radiography can be used to detect internal discontinuities in a casting. The discontinuities can be gas holes, non-metallic inclusions, shrinkage, cracks, inserts or chills or inclusions that have lower or higher densities than the parent metal. This document gives acceptance criteria through severity levels.

SIST EN 12681-1:2027 EN 12681-1:2026 (E)

1 Scope

This document gives specific procedures for industrial X-ray and gamma radiography for discontinuity detection purposes, using NDT (non-destructive testing) film techniques. This part of the EN 12681 series specifies the requirements for film radiographic testing of castings. Films after exposure and processing become radiographs with different area of optical density. Radiographs are viewed and evaluated using industrial radiographic illuminators. This part of the EN 12681 series specifies the recommended procedure for the choice of operating conditions and radiographic practice.

These procedures are applicable to castings produced by any casting process, especially for steel, cast iron, aluminium, cobalt, copper, magnesium, nickel, titanium, zinc and any alloys of them. NOTE This document considers EN ISO 5579.

This document does not apply to:

  • radiographic testing of castings for aerospace applications (see EN 2002-21);
  • radiographic testing of welded joints (see EN ISO 17636-1);
  • radiography with digital detectors (see EN 12681-2);
  • radioscopic testing (see the EN 13068 series).

2 Normative references

The following documents are referred to in the text in such a way that some or all of their content constitutes requirements of this document. For dated references, only the edition cited applies. For undated references, the latest edition of the referenced document (including any amendments) applies. EN ISO 5579:2013, Non-destructive testing — Radiographic testing of metallic materials using film and X- or gamma rays — Basic rules (ISO 5579:2013) EN ISO 5580, Non-destructive testing — Industrial radiographic illuminators — Minimum requirements (ISO 5580) EN ISO 9712, Non-destructive testing — Qualification and certification of NDT personnel (ISO 9712) EN ISO 11699-1, Non-destructive testing — Industrial radiographic film — Part 1: Classification of film systems for industrial radiography (ISO 11699-1) EN ISO 11699-2, Non-destructive testing — Industrial radiographic films — Part 2: Control of film processing by means of reference values (ISO 11699-2) EN ISO 19232-1, Non-destructive testing — Image quality of radiographs — Part 1: Determination of the image quality value using wire-type image quality indicators (ISO 19232-1) EN ISO 19232-2, Non-destructive testing — Image quality of radiographs — Part 2: Determination of the image quality value using step/hole-type image quality indicators (ISO 19232-2) ISO 5576, Non-destructive testing — Industrial X-ray and gamma-ray radiology — Vocabulary

SIST EN 12681-1:2027 EN 12681-1:2026 (E)

3 Terms and definitions

For the purposes of this document, the terms and definitions given in ISO 5576, EN ISO 5579 and the following apply.

ISO and IEC maintain terminology databases for use in standardization at the following addresses:

  • ISO Online browsing platform: available at https://www.iso.org/obp
  • IEC Electropedia: available at https://www.electropedia.org/

3.1 wall thickness

t thickness as measured on the casting

3.2 nominal wall thickness

t n thickness as specified on the drawing

3.3 penetrated thickness

w thickness of material in the direction of the radiation beam calculated on the basis of the real thicknesses of all penetrated walls

3.4 source size

d size of the radiation source or focal spot size [SOURCE: EN ISO 5579:2013, 3.4]

3.5 object-to-film distance

b largest (maximum) distance between the source side of the radiographed part of the test object and the film surface measured along the central axis of the radiation beam

3.6 source-to-object distance

f distance between the source of radiation and the source side of the test object, most distant from the film, measured along the central axis of the radiation beam

3.7 source-to-film distance

SFD distance between the source of radiation and the film measured in the direction of the beam Note 1 to entry: SFD = f + b where

SIST EN 12681-1:2027 EN 12681-1:2026 (E) f is the source-to-object distance; b is the object-to-film distance.

[SOURCE: EN ISO 5579:2013, 3.5, modified – description in words presented as formula]

4 Symbols and abbreviated terms

For the purposes of this document, the symbols and abbreviations apply:

b object-to-film distance d source size D optical density of film f source-to-object distance F film IQI image quality indicator S source of radiation SFD source-to film-distance t wall thickness t nominal wall thickness n w penetrated thickness

5 Classification of radiographic techniques

The radiographic techniques are divided into two testing classes:

  • Testing class A: basic techniques;
  • Testing class B: improved techniques.

It is recommended to perform the testing according to testing class A, if not otherwise specified in the order. Testing class B techniques are used when testing class A techniques are insufficiently sensitive. If, for technical or industrial reasons, it is not possible to meet one of the conditions specified for testing class B, such as the type of radiation source or the source-to-object distance f, it can be agreed by contracting parties that the condition selected may be what is specified for testing class A. In film radiography the loss of sensitivity shall be compensated by an increase of minimum optical density to 3,0 or by selection of a two class better film system. The other conditions for testing class B remain unchanged, especially the image quality achieved. Because of the better sensitivity compared to testing class A, the specimen may be regarded as being tested to testing class B. This does not apply if the special SFD reductions as specified in Clause 11 for test arrangements Figure 3 and Figure 4 are used.

SIST EN 12681-1:2027 EN 12681-1:2026 (E)

6 General preparations and requirements

6.1 General preparations

6.1.1 Protection against ionizing radiation

WARNING — Exposure of any part of the human body to X-rays or gamma-rays can be highly injurious to health. Wherever X-ray equipment or radioactive sources are in use, appropriate safety requirements shall be applied.

NOTE Local, national or international safety precautions are especially important to apply when using ionizing radiation.

6.1.2 Surface preparation and stage of manufacture

In general, surface preparation is not necessary, but where surface imperfections can cause difficulty in detecting discontinuities, the surface shall be ground smooth. Unless otherwise specified radiography shall be carried out after the final stage of manufacture, e.g. after grinding or heat treatment.

NOTE For some aluminium and magnesium alloy castings, radiography can be carried out before heat treatment.

6.2 Agreements

Castings with a complex geometry can include areas which cannot be tested by radiography or can only be partly tested. Such areas shall be identified before starting the radiographic testing. Areas which cannot be tested by radiography shall be noted by all contracting parties and be marked on the film position plan.

The following items shall be as agreed at the time of order:

a) manufacturing stage at which castings are to be tested; b) extent of radiographic testing; c) test areas; d) surface condition; e) testing class; f) information about the film position plan; g) marking of test areas on the casting; h) image quality; i) marking of the radiographs; j) acceptance criteria; k) any additional items; l) any special requirements.

SIST EN 12681-1:2027 EN 12681-1:2026 (E)

6.3 Personnel qualification

Unless otherwise agreed, testing shall be performed by personnel qualified in accordance with EN ISO 9712 or equivalent to an appropriate level in the relevant industrial sector.

7 Test arrangements

7.1 General

The test arrangements to be used shall be in accordance with:

Figure 1 to Figure 4: for single wall penetration; Figure 5 to Figure 7: for double wall penetration; Figure 8 to Figure 12: for test areas of complex section.

NOTE For an explanation of the symbols in the figures, see Clause 4. If these arrangements are not applicable, other arrangements may be used.

7.2 Single wall penetration of plane areas

The test arrangement for single wall penetration of plane areas shall be in accordance with Figure 1.

7.3 Single wall penetration of curved areas

The test arrangement for single wall penetration of curved areas shall be in accordance with either Figure 2, Figure 3 or Figure 4.

NOTE Rigid cassettes can be used if the corresponding increase of b is considered for the calculation of the distance f between the source and source side of the test object (see Clause 11).

7.4 Double wall penetration of plane and curved areas

The test arrangement for double wall penetration of plane and curved areas shall be in accordance with either Figure 5, Figure 6 or Figure 7.

In the case of test arrangements according to Figure 5, the distance of the source from the surface of the test area shall be minimized provided that the requirements of IQI are met. In the case of test arrangements according to Figure 6 and Figure 7, the discontinuities shall be classified with reference to the single wall thickness. In the case of different wall thicknesses the reference shall be the smaller one.

Double wall penetration shall be used, as an overview technique according to Figure 7, if the geometrical conditions make other test arrangements difficult to apply or if there is a better sensitivity for detecting discontinuities by using this technique. It shall be ensured that unacceptable discontinuities are detected with sufficient certainty. The required image quality shall be met.

7.5 Choice of test arrangements for complex geometries

Unless otherwise agreed, the test arrangements for complex geometry areas shall be in accordance with Figure 8 to Figure 12 (as appropriate).

SIST EN 12681-1:2027 EN 12681-1:2026 (E)

7.6 Acceptable test area dimensions

The test area to be captured with one radiographic film should be limited in a way that the required optical density according to Clause 12, Table 4 is met in the region of interest. In addition to the requirements above, the angle of incident radiation in the entire region of interest shall not exceed 30°.

NOTE This value can be larger, if special orientations of discontinuities can be detected in this way or if it is the only way to test areas otherwise impossible to test.

Figure 1 — Test arrangement for single wall penetration of plane areas

a) with flexible cassette

SIST EN 12681-1:2027 EN 12681-1:2026 (E)

b) with rigid cassette Figure 2 — Test arrangement for single wall penetration of curved areas with the source on the convex side and the film on the concave side of the test area

a) with flexible cassette

b) with rigid cassette Figure 3 — Test arrangement for single wall penetration of curved areas with eccentric positioning of the source on the concave side and the film on the convex side of the test area

SIST EN 12681-1:2027 EN 12681-1:2026 (E)

Figure 4 — Test arrangement for single wall penetration of curved areas with central positioning of the source on the concave side and film on the convex side of the test area

Figure 5 — Test arrangement for double wall penetration of plane or curved test areas; source and film outside the test area, only the film side wall imaged for evaluation

Figure 6 — Test arrangement for double wall penetration of plane or curved test areas; several exposures; source and film outside of the test area; both walls imaged for evaluation

SIST EN 12681-1:2027 EN 12681-1:2026 (E)

Figure 7 — Test arrangement for double wall penetration of plane or curved test areas; overview exposure; source and film outside of the test area; both walls imaged for evaluation

a) standard arrangement

b) alternative arrangement b) should only be used if a) is not possible.

Figure 8 — Test arrangements for edges and flanges

SIST EN 12681-1:2027 EN 12681-1:2026 (E)

a) standard arrangement

b) alternative arrangement b) should only be used if a) is not possible.

Figure 9 — Test arrangements for ribs

Figure 10 — Test arrangement for cross like geometries

SIST EN 12681-1:2027 EN 12681-1:2026 (E)

Figure 11 — Test arrangement for wedge geometries

a) for supports

b) for ribs Figure 12 — Test arrangement for ribs and supports

SIST EN 12681-1:2027 EN 12681-1:2026 (E)

8 Choice of tube potential and radiation source

8.1 X-ray devices up to 1 000 kV

To maintain good detection sensitivity, the X-ray tube potential (voltage) should be as low as possible. The maximum values of X-ray tube potential versus thickness are given in Figure 13. NOTE The calculations for the curves in Figure 13 are described in Annex G.

Key 1 copper/nickel and alloys 4 aluminium and alloys 2 steel and cast irons w penetrated thickness in mm 3 titanium and alloys U X-ray potential in kV Figure 13 — Maximum X-ray potential U for X-ray devices up to 1 000 kV as a function of penetrated thickness w and material For some casting applications where the thickness changes across the area of test object being radiographed, a modification of technique with a higher potential may be used, but it should be noted that an excessively high tube potential will lead to a loss of detection sensitivity. If there are different thicknesses imaged with one exposure, an averaged value of these thicknesses can be used.

8.2 Other radiation sources

The penetrated thickness ranges for gamma ray sources and X-ray potentials higher than 1 MV are given in Table 1 for steels, cast irons, cobalt, copper and nickel based alloys. For aluminium, magnesium, titanium and zinc testing using Se 75, the penetrated material thickness is 35 mm ≤ w ≤ 120 mm for testing class A.

SIST EN 12681-1:2027 EN 12681-1:2026 (E) Gamma rays from Se 75, Ir 192 and Co 60 sources will not produce radiographs having as good detection sensitivity as X-rays used with appropriate technique parameters. However, because of the advantages of gamma ray sources in handling and accessibility, Table 1 gives a range of thicknesses for which each of these gamma ray sources may be used when the use of X-ray tubes is difficult. By agreement between the contracting parties, the penetrated material thickness for Ir 192 may be further reduced to 10 mm.

By agreement between the contracting parties, the penetrated material thickness for Se 75 may be further reduced for testing class A or testing class B, provided the required image quality as stated in Clause 16 is achieved. It is recommended that better film system classes are used for testing of penetrated thicknesses below 10 mm with Se 75 than required in Tables 2 and 3. For certain applications wider material thickness ranges may be permitted, if sufficient image quality can be achieved.

For gamma rays, the total travel-time to and from the source position shall not exceed 10 % of the total exposure time.

Table 1 — Penetrated thickness range for gamma ray sources and X-ray equipment with X-ray potential above 1 MV for steels, cast irons, cobalt, copper and nickel base alloys Penetrated thickness a w Radiation source mm Testing class A Testing class B Se 75 10 ≤ w ≤ 40 14 ≤ w ≤ 40 Ir 192 10 ≤ w ≤ 100 20 ≤ w ≤ 90 Co 60 40 ≤ w ≤ 200 60 ≤ w ≤ 150 X-ray potentials from 1 MV up to 4 MV 30 ≤ w ≤ 300 50 ≤ w ≤ 180 b b X-ray potentials from 4 MV up to 12 MV w ≥ 50 w ≥ 70 b b X-ray potentials above 12 MV w ≥ 80 w ≥ 100 a If there are different thicknesses imaged with one exposure, an averaged value of these thicknesses can be used.

b The minimum penetrated wall thickness may be reduced by 10 mm in testing class A and by 20 mm in testing class B, if film system class C1 according to EN ISO 11699-1 is used, provided the IQI requirements are met.

9 Film systems and metal screens

For radiographic testing, film system classes shall be used in accordance with EN ISO 11699-1. For different radiation sources, the minimum film system classes are given in Table 2 and Table 3. When using metal screens good contact between films and screens is required. This shall be achieved either by using vacuum-packed films or by applying pressure.

Other screen thicknesses may be also used provided the required image quality is achieved.

SIST EN 12681-1:2027 EN 12681-1:2026 (E) Table 2 — Film system classes and metal screens for the radiography of steels, cast irons, cobalt, copper and nickel base alloys Film system Penetrated thickness Type and thickness of metal screens a class Radiation source Testing Testing w Testing class A Testing class B class A class B none or up to 0,03 mm front and back X-ray potentials ≤ 100 kV screens of lead C 3 100 kV < X-ray up to 0,15 mm front and back screens of all w C 5 potentials ≤ 150 kV lead 150 kV < X-ray 0,02 mm to 0,15 mm front and back C 4 potentials ≤ 250 kV screens of lead 0,02 mm to 0,2 mm front and back screens w ≤ 50 mm C 4 of lead 250 kV < X-ray C 5 b potentials ≤ 500 kV 0,1 mm to 0,2 mm front screens of lead w > 50 mm C 5 0,02 mm to 0,2 mm back screens of lead w ≤ 75 mm C 5 C 4 500 kV < X-ray 0,25 mm to 0,7 mm front and back screens

potentials ≤ 1 000 kV of steel or copper w > 75 mm C 5 C 5 0,02 mm to 0,2 mm front and back screens Se 75 all w C 5 C 4 of lead 0,1 mm to 0,2 mm 0,02 mm to 0,2 mm front screens of lead front screens of lead Ir 192 all w C 5 C 4 b

0,02 mm to 0,2 mm back screens of lead w ≤ 100 mm C 4 0,25 mm to 0,7 mm front and back screens Co 60 C 5

of steel or copper w > 100 mm C 5 w ≤ 100 mm C 3

1 MV < X-ray 0,25 mm to 0,7 mm front and back screens

C 5

potentials ≤ 4 MV of steel or copper w > 100 mm C 5 up to 1 mm front screen of copper, steel or w ≤ 100 mm C 4 C 2 d tantalum

4 MV < X-ray

100 mm < w ≤ 300 mm C 4

potentials ≤ 12 MV back screen of copper or steel up to 1 mm C 5 d w > 300 mm C 5 or tantalum up to 0,5 mm e w ≤ 100 mm C 4 C 1 up to 1 mm front screen of tantalum No back screen X-ray potentials above 100 mm < w ≤ 300 mm C 3 12 MV C 5 e up to 1 mm front screen of tantalum up w > 300 mm C 5 to 0,5 mm back screen of tantalum a Better film system classes may also be used according to EN ISO 11699-1. b Ready packed films with a front screen up to 0,03 mm may be used if an additional lead screen of 0,1 mm is placed between the test object and the film.

In testing class A also 0,5 mm to 2,0 mm screens of lead may be used. d In testing class A lead screens 0,5 mm to 1 mm may be used by agreement between the contracting parties. e Tungsten screens may be used by agreement.

SIST EN 12681-1:2027 EN 12681-1:2026 (E) Table 3 — X-ray potentials, film system classes and metal screens for aluminium, magnesium, titanium and zinc a Film system class Type and thickness of intensifying Radiation source Testing Testing screens class A class B none or up to 0,03 mm front and up to X-ray potentials ≤ 150 kV 0,15 mm back screens of lead 0,02 mm to 0,15 mm front and back 150 kV < X-ray potentials ≤ 250 kV C 3 screens of lead C 5 0,1 mm to 0,2 mm front and back screens 250 kV < X-ray potentials ≤ 500 kV of lead b not 0,2 mm front and 0,1 mm to 0,2 mm back Se 75 applicable screens of lead a Better film system classes may also be used, see EN ISO 11699-1. b Instead of one 0,2 mm lead screen, two 0,1 mm lead screens may be used.

10 Reduction of scattered radiation

10.1 Metal filters and collimators

In order to reduce the effect of scattered radiation, direct radiation shall be collimated as much as possible to the section under examination.

...