ISO 25408-1
(Main)Testing method for bead wire — Part 1: General requirements
- Abstract
This document specifies test methods of round steel Bead Wires which are used for tyre reinforcement.Test methods on Mechanical properties and Chemical properties (coating analysis) are included. By agreement, these test methods may be applied to similar single filaments used for reinforcing other rubber products.
- Status
- Not Published
- Technical Committee
- ISO/TC 17/SC 17 - Steel wire rod and wire products
- Drafting Committee
- ISO/TC 17/SC 17/WG 22 - Testing method for bead wire
- Current Stage
- 6000 - International Standard under publication - 60 Publication
- Start Date
- 22-Oct-2026
Buy Documents
ISO/FDIS 25408-1 - Testing method for bead wire — Part 1: General requirements
REDLINE ISO/FDIS 25408-1 - Testing method for bead wire — Part 1: General requirements
ISO 25408-1 is an ISO standard for testing round steel bead wires used for tyre reinforcement. It specifies test methods for mechanical properties and chemical properties, including coating analysis, and it may also be applied by agreement to similar single filaments used to reinforce other rubber products.
What does ISO 25408-1 specify?
ISO 25408-1 specifies the test methods used to check bead wire diameter, tensile behavior, bend performance, torsion behavior, residual torsion, straightness, tip rise, S-shape, and bronze coating by X-ray fluorescence spectroscopy (XRFS). These methods are intended for round steel bead wires used in tyre reinforcement, with agreed use allowed for similar reinforcing filaments in other rubber products.
The document is organized in clauses 1 to 11. It starts with scope, normative references, and terms and definitions, then gives separate method clauses for diameter, tensile testing, reverse bend testing, torsion testing, residual torsions, straightness, tip rise and S-shape checks, and bronze coating analysis.
What are the key requirements of ISO 25408-1?
ISO 25408-1 gives practical test setups and reporting rules so different laboratories can compare bead wire results in a consistent way. The most important requirements are the defined measurement methods, the test conditions, and the way results are reported.
Diameter measurement
ISO 25408-1 gives two diameter methods in Clause 4: micrometre measurement and non-contact laser measurement. The micrometre method requires a precision outside micrometre with 0.001 mm resolution, a circular spindle, and careful zero-setting before each test series.
In practice, the wire must be clean, as straight as possible at the measured area, and measured with gentle closing force. The standard also defines how to calculate average diameter and out-of-roundness from repeated readings. This matters because diameter control is a basic acceptance check for bead wire consistency.
Tensile testing
ISO 25408-1 Clause 5 covers maximum force, total elongation at fracture, and yield ratio from a constant rate of extension tensile test. The wire is clamped under defined pretension and loaded until fracture, producing a force-extension curve from which the results are calculated.
The standard specifies machine features, grip types, optional extensometers, and test speeds. It also sets limits for invalid results, such as fracture in or very near the grip area, and it gives reporting precision for force, tensile strength, elongation, and yield ratio. In practice, this tells the tester how to set up the machine and when a result must be repeated.
Bend testing
ISO 25408-1 Clause 6 describes the reverse bend test used to judge plastic deformation capability under alternating bending. The wire is bent alternately left and right over defined supports until fracture occurs.
The test uses a bend tester with dimensions selected according to wire diameter, and the bending rate shall not exceed one reverse bend per second unless otherwise specified. The result is the complete number of reverse bends to fracture. This is a direct way to compare flexibility and durability of bead wire under repeated bending.
Torsion testing
ISO 25408-1 Clause 7 covers simple torsion testing of a single wire filament. One end is fixed, the other is rotated until fracture or until a specified number of turns is reached.
The standard requires suitable grips, controlled axial load, defined test length rules, and standard aging when requested. It also states when a result is valid or invalid based on fracture location and torsion in the clamp area. This matters because torsion performance is a key indicator of wire formability and internal quality.
Residual torsion, straightness, tip rise, and shape
ISO 25408-1 Clauses 8, 9, and 10 cover geometric and handling-related checks. Clause 8 measures residual torsions by unwinding a 6 m length and counting the revolutions of the free end after a 90° bend is released.
Clause 9 provides two straightness options: a 3 m parallel-line check or an arc height method. Clause 10 adds visual checks for tip rise and for S-shape or C-shape during the residual torsion check. In practice, these checks show whether the wire will lay and handle properly in later processing.
Bronze coating by XRFS
ISO 25408-1 Clause 11 describes bronze coating mass and composition measurement by XRFS. The wire sample is prepared in a holder, the instrument is calibrated, and coating mass and tin fraction are calculated from the measured copper and tin signals.
The test report gives tin mass fraction and coating mass with specified rounding. This is important for confirming the coating condition of bead wire, which affects performance and consistency in use.
What terms does ISO 25408-1 define?
- Diameter - the average of the maximum and minimum values from multiple transverse measurements on the same section of the specimen.
- Out-of-roundness - the absolute difference between the maximum and minimum diameter measured in the same transverse cross-section.
- Maximum force (Fm) - the highest load the material withstands in the static tensile test; it is not the same as breaking load.
- Total elongation at fracture - the elongation at break expressed as a percentage of the original gauge length.
- Yield ratio - the force ratio at 0.2 % elongation offset to maximum force, expressed in percent.
- Tensile strength (Rm) - maximum force divided by the original cross-sectional area.
- Arc height - a practical expression of the short-distance straightness of bead wire.
- Straightness - the maximum bow height, or curvature, measured over a given gauge length of the wire.
Who uses ISO 25408-1?
ISO 25408-1 is used by bead wire manufacturers, tyre reinforcement suppliers, and laboratories that test wire properties for production control or product release. Quality managers use it to define how to measure diameter, tensile properties, bend behavior, torsion, straightness, and coating condition in a repeatable way.
It is also relevant to buyers and technical teams in the tyre and rubber product supply chain. For them, the standard provides a common basis for comparing supplier data and for agreeing on test conditions when similar single filaments are used for other rubber products.
Which standards are used with ISO 25408-1?
ISO 25408-1 cites two normative references that support its test methods:
- ISO 7800:2012 - provides the simple torsion test method and is also referenced for fracture evaluation in Clause 7.
- ISO 16650:2025 - provides the bead wire reference used in the terminology and supports the elongation-at-fracture definition.
What does the ISO 25408-1 document contain?
ISO 25408-1 contains worked test methods, apparatus descriptions, procedures, calculation formulas, and reporting rules for bead wire testing. It includes figures for the micrometre setup, bend tester, tensile curve, reverse bend arrangement, residual torsion setup, straightness checks, arc height setup, and tip rise and S-shape evaluation.
The document also includes Table 1 for acceptable coefficient of variation in tensile results, Table 2 for bend device parameters, Table 3 for bend repeatability, Table 4 for torsion repeatability, and Table 5 with example XRFS calibration standards. These tables support laboratory control, method selection, and comparison of results.
Clause 5 includes formulas and software functions for tensile calculations, Clause 4 includes formulas for diameter and out-of-roundness, and Clause 11 includes formulas for coating mass and tin fraction. In practice, these parts are used for testing, quality control, and result reporting rather than for design rules.
Buy Documents
ISO/FDIS 25408-1 - Testing method for bead wire — Part 1: General requirements
REDLINE ISO/FDIS 25408-1 - Testing method for bead wire — Part 1: General requirements
Get Certified
Connect with accredited certification bodies for this standard
DIN CERTCO
DIN Group product certification.

Element Materials Technology
Materials testing and product certification.

Inštitut za kovinske materiale in tehnologije
Institute of Metals and Technology. Materials testing, metallurgical analysis, NDT.
Sponsored listings
Frequently Asked Questions
ISO 25408-1 is a draft published by the International Organization for Standardization (ISO). Its full title is "Testing method for bead wire — Part 1: General requirements". This standard covers: This document specifies test methods of round steel Bead Wires which are used for tyre reinforcement.Test methods on Mechanical properties and Chemical properties (coating analysis) are included. By agreement, these test methods may be applied to similar single filaments used for reinforcing other rubber products.
This document specifies test methods of round steel Bead Wires which are used for tyre reinforcement.Test methods on Mechanical properties and Chemical properties (coating analysis) are included. By agreement, these test methods may be applied to similar single filaments used for reinforcing other rubber products.
ISO 25408-1 is classified under the following ICS (International Classification for Standards) categories: 77.140.65 - Steel wire, wire ropes and link chains; 83.140.01 - Rubber and plastics products in general; 83.160.01 - Tyres in general. The ICS classification helps identify the subject area and facilitates finding related standards.
ISO 25408-1 is available in PDF format for immediate download after purchase. The document can be added to your cart and obtained through the secure checkout process. Digital delivery ensures instant access to the complete standard document.
Standards Content (Sample)
Contents
- 1 Scope
- 2 Normative references
- 3 Terms and definitions
- 3.1 diameter
- 3.2 out-of-roundness
- 3.3 maximum force
- 3.4 total elongation at fracture
- 3.5 yield strength
- 3.6 yield ratio
- 3.7 tensile strength
- 3.8 arc height
- 3.9 straightness
- 4 Diameter
- 4.1 Measuring with micrometre
- 4.2 Non contact methods — Laser
- 5 Maximum force, total elongation at fracture and yield ratio
- 5.1 Principle
- 5.2 Apparatus
- 5.3 Test procedure
- 5.4 Calculation
- 5.5 Report
- 5.6 Precision and variance limits
- 6 Bend
- 6.1 Principle
- 6.2 Apparatus
- 6.3 Test procedure
- 6.4 Report
- 6.5 Precision and variance
- 7 Torsions
- 7.1 Principle
- 7.2 Apparatus
- 7.3 Test procedure
- 7.4 Report
- 7.5 Precision and variance
- 8 Residual torsions bead wire
- 8.1 Principle
- 8.2 Apparatus
- 8.3 Test procedure
- 8.4 Report
- 9 Straightness
- 9.1 Principle
- 9.4 Report
- 10 Tip rise and S-shape of bead wire
- 10.1 Test procedures
- 10.2 Report
- 10.3 S-shape of bead wire
- 10.4 Report
- 11 Mass and composition of bronze coating by X-ray fluorescence spectroscopy
- 11.1 Principle
- 11.2 Apparatus
- 11.3 Test procedure
- 11.4 Expression of results
- 11.5 Test report
- Bibliography
1 Scope
This document specifies test methods of round steel bead wires (BW) which are used for tyre reinforcement. Test methods on mechanical properties and chemical properties (coating analysis) are included. By agreement, these test methods can be applied to similar single filaments used for reinforcing other rubber products.
2 Normative references
The following documents are referred to in the text in such a way that some or all of their content constitutes requirements of this document. For dated references, only the edition cited applies. For undated references, the latest edition of the referenced document (including any amendments) applies. ISO 7800:2012, Metallic materials — Wire — Simple torsion test
3 Terms and definitions
For the purposes of this document, the following terms and definitions apply. ISO and IEC maintain terminology databases for use in standardization at the following addresses:
- ISO Online browsing platform: available at https:// www .iso .org/ obp
- IEC Electropedia: available at https:// www .electropedia .org/
3.1 diameter
average of maximum and minimum values in multiple transversal measurements on the same section of the specimen.
3.2 out-of-roundness
absolute value of the arithmetic difference between the maximum and minimum diameter measured in the same transverse cross-section perpendicular to the wire axis
3.3 maximum force
F m highest load that the material withstands when subjected to the static tensile test is represented, expressed in newtons Note 1 to entry: Maximum force is not equal to breaking load.
ISO/FDIS 25408-1:2026(en)
3.4 total elongation at fracture
percentage of the ratio of the arithmetic value of subtracting the original gauge length from the total length of the specimen at the time of fracture to the original gauge length [SOURCE: ISO 16650:2025,3.4] Note 1 to entry: Total elongation at fracture is not equal to Total elongation at maximum force.
3.5 yield strength
highest stress to which a material can be subjected before plastic deformation occurs
3.6 yield ratio
force ratio at 0,2 % elongation offset to maximum force, expressed in %
3.7 tensile strength
R m maximum force, F , that the test piece withstands divided by the original cross-sectional area, expressed in m
N/mm
3.8 arc height
expression of short distance for straightness of bead wire Note 1 to entry: It is a more practical and easier way of working to determine the performance of straightness of bead wire
3.9 straightness
maximum bow height (or curvature) measured over a given gauge length of the wire
4 Diameter
4.1 Measuring with micrometre
4.1.1 Principle
Hold the sample between two parallel circular faced anvils of a micrometre. Close the movable anvil gradually and gently until it is in contact with the specimen. Read the value on the micrometre.
4.1.2 Apparatus
4.1.2.1 Micrometre
a) A precision cylindrical outside micrometre with non-rotating spindle type with a resolution of 0,001 mm shall be used (see Figure 1).
b) The micrometre shall have a circular spindle of ⌀6,35 mm in diameter. c) Measuring range of the micrometre is from 0 mm to 25 mm.
d) Measuring force range of the micrometre is <10 N.
ISO/FDIS 25408-1:2026(en) Figure 1 — Micrometre illustration
4.1.3 Test procedure
4.1.3.1 Sample preparation
a) Cut a sample at length (about 10 cm to 15 cm).
b) A right-angle bend on the wire is to be applied to assist in rotating the wire between measurements. c) The measured area of the wire shall be as straight as possible. d) The wire surface shall be clean. Dirt and lubricant residues shall be removed with a clean tissue.
4.1.3.2 Zero-setting of the micrometre
a) Check the zero position of the micrometre and ensure that the numerical value displayed is 0,000 with closed anvils for electronic micrometre, for a mechanical micrometre, the zero graduation line of the fixed sleeve shall be aligned.
b) If reset action is needed, both anvil faces shall always be cleaned with a clean paper prior to the reset action.
c) This ‘zero-setting’ procedure shall to be done before each test series.
4.1.3.3 Method of measuring
a) The movable anvil is closed until it is in contact with the specimen. Closing speed shall be controlled until three clicks can be heard. The closing speed shall be controlled to avoid too high closing pressure. b) Measure at least three values at the one section. Record the maximum as d and minimum as d or 1 2 measure two values in two perpendicular directions at the same cross-section, and record two values as d and d .
3 4
4.1.4 Calculations and report
4.1.4.1 Method for diameter
Determine the wire diameter by calculating the arithmetic mean (AVG) of maximum and minimum with Formula (1):
ISO/FDIS 25408-1:2026(en)
d = (d + d )/2 (1) 0 1 2 where d is the average diameter, expressed in millimetres (mm);
d is the maximum diameter, expressed in millimetres (mm);
d is the minimum diameter, expressed in millimetres (mm).
or determine the wire diameter by calculating the arithmetic average of two measured values with Formula (2) d = (d + d )/2 (2) 0 3 4 where d is the average diameter, expressed in millimetres (mm);
d is one diameter measured in perpendicular directions, expressed in millimetres (mm);
d is the other diameter measured in perpendicular directions, expressed in millimetres (mm)
4.1.4.2 Method for out-of-roundness
Determine the ‘out-of-roundness’ by calculating the difference of the two readings with Formula (3). O= d – d (3) 1 2 where O is the out-of-roundness or ovality of wire, expressed in millimetres (mm); d is the maximum diameter, expressed in millimetres (mm);
d is the minimum diameter, expressed in millimetres (mm).
4.2 Non contact methods — Laser
a) A minimum resolution of 0,001 mm is required.
b) The sample shall be cleaned prior to the test.
c) During the measurement, the sample shall be perpendicular to the direction in which the laser is emitted.
d) The sample shall be rotatable during testing to have multiple measurements to calculate the average diameter. The out-of-roundness or non-contact measuring device shall be able to test in multiple angles (Min 4) to take average diameter and roundness.
NOTE Rotating sample or working with multiple angles laser are all acceptable.
5 Maximum force, total elongation at fracture and yield ratio
5.1 Principle
Both ends of a test sample are clamped under a defined pretension in a tensile testing machine; increasing load under a constant rate of extension is applied until the specimen breaks. The change in force is measured versus the increase in separation of the specimen clamps to form a force-extension curve. The maximum force is measured, total elongation at fracture and yield ratio are calculated (see Figure 2). NOTE The auto-calculated Young’s modulus is taken to form modulus line for calculating the R proof of P0,2 strength or yield strength.
ISO/FDIS 25408-1:2026(en) Key F force 0 zero point curve e percentage extension F maximum force m R proof strength, plastic extension p e specified percentage plastic extension p m slope of the elastic part of the stress-percentage extension E a fracture A percentage total extension at fracture t Figure 2 — Tensile stress-strain curve
5.2 Apparatus
5.2.1 Tensile testing machine
a) For the constant rate of extension (CRE) tensile testing machine, the measured force required to fracture the wire shall not exceed 90 % of the selected force measurement range. The device is equipped with a load and extension recorder, digital read-out, automated data logger or computer controlled tensile test machine.
b) The cross-head speed: maximum speed ≥ 150 mm/min. (≠ test speed) c) The machine accuracy Class 0,5 = Load weighing accuracy: ± 0,5 % d) The load cell capacity depends on the type and characteristics of the wire. e) The structure of the machine and gripping systems shall be able to handle the axial force. f) The specifications and methods of calibration and verification for tensile testing machines shall conform to appropriate standards.
5.2.2 Grips
Grip types shall be selected according to the wire dimensions and characteristics and within range of the load cell. They may be wedge grip type or action screw type or pneumatic action type with suitable jaw faces (serrated or grooved) to avoid failure of specimen at gripping point and avoid slippage of specimen within the jaws (grips).
ISO/FDIS 25408-1:2026(en)
5.2.3 Extensometer (Optional)
a) Contact or non-contact extensometers.
b) Resolution of 0,001 % of the gauge length.
c) Gauge length: length = 200 mm (≠ test length) or according to customer requirements. d) Extensometer accuracy Class 0,5 - Contact extensometer with sensor and contact arms - Non-contact extensometer e) Video extensometer f) Laser extensometer g) Light extensometer
5.2.4 Oven (Optional)
- Specifications : Capable of reaching temperatures up to 200 °C.
- Built-in timer is preferred.
5.3 Test procedure
5.3.1 Sample preparation
a) The sample taking process shall avoid any undulations, loops, bends or damage of the wire and wire surface. The sample shall be as straight as possible.
b) Cut a piece of wire of the used test length plus twice the length of a jaw face. c) L + 2x clamping length.
o d) When slippage occurs in the clamps a new sample shall be taken to retest. e) When requested, the wire can be thermally aged in an oven. Aging time and aging temperature as agreed with requester. Standard aging conditions are: 60 min ± 1 min at 150 °C ± 3 °C.
5.3.2 Test procedure
5.3.2.1 Test settings
a) Test length:
- Original gauge length is L , standard extensometer gauge length is L ; o e
- The gauge length L can be adjusted on customer request.
...
Contents
- 1 Scope
- 2 Normative references
- 3 Terms and definitions
- 4 Diameter
- 4.1 Measuring with micrometre
- 4.2 Non contact methods –— Laser
- 5 Maximum force, total elongation at fracture and yield ratio
- 5.1 Principle
- 5.2 Apparatus
- 5.3 Test procedure
- 5.4 Calculation
- 5.5 Report
- 5.6 Precision and variance limits
- 6 Bend
- 6.1 Principle
- 6.2 Apparatus
- 6.3 Test procedure
- 6.4 Report
- 6.5 Precision and variance
- 7 Torsions
- 7.1 Principle
- 7.2 Apparatus
- 7.3 Test procedure
- 7.4 Report
- 7.5 Precision and variance
- 8 Residual torsions bead wire
- 8.1 Principle
- 8.2 Apparatus
- 8.3 Test procedure
- 8.3 Test procedure
- 8.4 Report
- 9 Straightness
- 9.1 Principle
- 9.4 Report
- 10 Tip rise and S-shape of bead wire
- 10.1 Test procedures
- 10.2 Report
- 10.3 S-shape of bead wire
- 10.4 Report
- 11 Mass and composition of bronze coating by X-ray fluorescence spectroscopy
- 11.1 Principle
- 11.2 Apparatus
- 11.3 Test procedure
- 11.4 Expression of results
- 11.5 Test report
- Bibliography
1 Scope
This document specifies test methods of round steel bead wires (BW) which are used for tyre reinforcement. Test methods on mechanical properties and chemical properties (coating analysis) are included. By agreement, these test methods maycan be applied to similar single filaments used for reinforcing other rubber products.
2 Normative references
The following documents are referred to in the text in such a way that some or all of their content constitutes requirements of this document. For dated references, only the edition cited applies. For undated references, the latest edition of the referenced document (including any amendments) applies. ISO 7800:2012, Metallic materials — Wire — Simple torsion test ISO 16650:2025, Bead wire
3 Terms and definitions
For the purposes of this document, the following terms and definitions apply. ISO and IEC maintain terminology databases for use in standardization at the following addresses:
- — ISO Online browsing platform: available at https://www.iso.org/obp
- — IEC Electropedia: available at https://www.electropedia.org/ 3.1 3.1 diameter average of maximum and minimum values in multiple transversal measurements on the same section of the specimen.
3.2 3.2 out-of-roundness absolute value of the arithmetic difference between the maximum and minimum diameter measured in the same transverse cross-section perpendicular to the wire axis 3.3 3.3 maximum force F m highest load that the material withstands when subjected to the static tensile test is represented, expressed in newtons Note 1 to entry: Maximum force is not equal to breaking load.
ISO/FDIS 25408-1:2026(en) 3.4 3.4 total elongation at fracture percentage of the ratio of the arithmetic value of subtracting the original gauge length from the total length of the specimen at the time of fracture to the original gauge length [SOURCE: ISO 16650:2025,3.4] Note 1 to entry: Total elongation at fracture is not equal to Total elongation at maximum force. 3.5 3.5 yield strength highest stress to which a material can be subjected before plastic deformation occurs 3.6 3.6 yield ratio force ratio at 0,2 % elongation offset to maximum force, expressed in % 3.7 3.7 tensile strength R m maximum force, Fm, that the test piece withstands divided by the original cross-sectional area, expressed in
N/mm 3.8 3.8 arc height expression of short distance for straightness of bead wire Note 1 to entry: It is a more practical and easier way of working to determine the performance of straightness of bead wire 3.9 3.9 straightness maximum bow height (or curvature) measured over a given gauge length of the wire
4 Diameter
4.1 Measuring with micrometre
4.1.1 Principle
Hold the sample between two parallel circular faced anvils of a micrometre. Close the movable anvil gradually and gently until it is in contact with the specimen. Read the value on the micrometre.
4.1.2 Apparatus
4.1.2.1 4.1.2.1 Micrometre a) a) A precision cylindrical outside micrometre with non-rotating spindle type with a resolution of 0,001 mm shall be used (see Figure 1Figure 1).).
b) b) The micrometre shall have a circular spindle of ⌀6,35 mm in diameter. c) c) Measuring range of the micrometre is from 0 mm to 25 mm. d) d) Measuring force range of the micrometre is <10 N.
ISO/FDIS 25408-1:2026(en)
Figure 1 — Micrometre illustration
4.1.3 Test procedure
4.1.3.1 Sample preparation
a) a) Cut a sample at length (about 10 cm to 15 cm).
b) b) A right-angle bend on the wire is to be applied to assist in rotating the wire between measurements.
c) c) The measured area of the wire shall be as straight as possible. d) d) The wire surface shall be clean. Dirt and lubricant residues shall be removed with a clean tissue.
4.1.3.2 Zero-setting of the micrometre
a) a) Check the zero position of the micrometre and ensure that the numerical value displayed is 0,000 with closed anvils for electronic micrometre, for a mechanical micrometre, the zero graduation line of the fixed sleeve shall be aligned.
b) b) If reset action is needed, both anvil faces shall always be cleaned with a clean paper prior to the reset action.
c) c) This ‘zero-setting’ procedure shall to be done before each test series.
ISO/FDIS 25408-1:2026(en)
4.1.3.3 Method of measuring
a) a) The movable anvil is closed until it is in contact with the specimen. Closing speed shall be controlled until three clicks can be heard. The closing speed shall be controlled to avoid too high closing pressure.
b) b) Measure at least three values at the one section. Record the maximum as d and minimum as
d2 or measure two values in two perpendicular directions at the same cross-section, and record two values as d and d .
3 4
4.1.4 Calculations and report
4.1.4.1 Method for diameter
Determine the wire diameter by calculating the arithmetic mean (AVG) of maximum and minimum with Formula (1)Formula (1)::
d =( = (d + d )/2 (1) 0 1 2 where d is the average diameter, expressed in millimetres (mm);
d is the maximum diameter, expressed in millimetres (mm);
d2 is the minimum diameter, expressed in millimetres (mm).
or determine the wire diameter by calculating the arithmetic average of two measured values with Formula (2)Formula (2) d = (d + d )/2 (2) 0 3 4 where d0 is the average diameter, expressed in millimetres (mm); d3 is one diameter measured in perpendicular directions, expressed in millimetres (mm); d4 is the other diameter measured in perpendicular directions, expressed in millimetres (mm)
4.1.4.2 Method for out-of-roundness
Determine the ‘out-of-roundness’ by calculating the difference of the two readings with Formula (3)Formula (3)..
O= d – d (3) 1 2 where O is the out-of-roundness or ovality of wire, expressed in millimetres (mm); d is the maximum diameter, expressed in millimetres (mm);
d2 is the minimum diameter, expressed in millimetres (mm).
4.2 Non contact methods –— Laser
a) a) A minimum resolution of 0,001 mm is required.
b) b) The sample shall be cleaned prior to the test.
c) c) During the measurement, the sample shall be perpendicular to the direction in which the laser is emitted.
ISO/FDIS 25408-1:2026(en) d) d) The sample shall be rotatable during testing to have multiple measurements to calculate the average diameter. The out-of-roundness or non-contact measuring device shall be able to test in multiple angles (Min 4) to take average diameter and roundness.
NOTE Rotating sample or working with multiple angles laser are all acceptable.
5 Maximum force, total elongation at fracture and yield ratio
5.1 Principle
Both ends of a test sample are clamped under a defined pretension in a tensile testing machine; increasing load under a constant rate of extension is applied until the specimen breaks. The change in force is measured versus the increase in separation of the specimen clamps to form a force-extension curve. The maximum force is measured, total elongation at fracture and yield ratio are calculated (see Figure 2Figure 2).). NOTE The auto-calculated Young’s modulus is taken to form modulus line for calculating the R . proof of strength P0 ,2 or yield strength.
ISO/FDIS 25408-1:2026(en)
Key F force 0 zero point curve e percentage extension Fm maximum force Rp proof strength, plastic extension ep specified percentage plastic extension 0 zero point mE slope of the elastic part of the stress-percentage extension curve e percentage extension a fracture Fm maximum force At percentage total extension at fracture Rp proof strength, plastic extension
Figure 2 — Tensile stress-strain curve
ISO/FDIS 25408-1:2026(en)
5.2 Apparatus
5.2.1 Tensile testing machine
a) a) For the constant rate of extension (CRE) tensile testing machine, the measured force required to fracture the wire shall not exceed 90 % of the selected force measurement range. The device is equipped with a load and extension recorder, digital read-out, automated data logger or computer controlled tensile test machine.
b) b) The cross-head speed: maximum speed ≥ 150 mm/min. (≠ test speed) c) c) The machine accuracy Class 0,5 = Load weighing accuracy: +/-± 0,5 % d) d) The load cell capacity depends on the type and characteristics of the wire. e) e) The structure of the machine and gripping systems shall be able to handle the axial force. f) f) The specifications and methods of calibration and verification for tensile testing machines shall conform to appropriate standards...
5.2.2 Grips
Grip types shall be selected according to the wire dimensions and characteristics and within range of the load cell. They may be wedge grip type or action screw type or pneumatic action type with suitable jaw faces (serrated or grooved) to avoid failure of specimen at gripping point and avoid slippage of specimen within the jaws (grips).
5.2.3 Extensometer (Optional)
a) a) Contact or non-contact extensometers.
b) b) Resolution of 0,001 % of the gauge length.
c) c) Gauge length: length = 200 mm (≠ test length) or according to customer requirements. d) d) Extensometer accuracy Class 0,5 - — Contact extensometer with sensor and contact arms - — Non-contact extensometer e) e) Video extensometer f) f) Laser extensometer g) g) Light extensometer
5.2.4 Oven (Optional)
- — Specifications : Capable of reaching temperatures up to 200 °C.
- — Built-in timer is preferred.
ISO/FDIS 25408-1:2026(en)
5.3 Test procedure
5.3.1 Sample preparation
a) a) The sample taking process shall avoid any undulations, loops, bends or damage of the wire and wire surface. The sample shall be as straight as possible.
b) b) Cut a piece of wire of the used test length plus twice the length of a jaw face. c) c) L + 2x clamping length.
o d) d) When slippage occurs in the clamps a new sample shall be taken to retest. e) e) When requested, the wire can be thermally aged in an oven. Aging time and aging temperature as agreed with requester. Standard aging conditions are: 60 min ± 1 min at 150 °C ± 3 °C.
5.3.2 Test procedure
5.3.2.1 Test settings:
a) a) Test length:
- — Original gauge length is Lo, standard extensometer gauge length is Le;
- — The gauge length L can be adjusted on customer request.
o - — Standard extensometer gauge length is L : = 200 mm e b) b) Speed:
...