ISO 14577-1:2026
(Main)Metallic materials — Instrumented indentation test for hardness and materials parameters — Part 1: Test method
- Abstract
This document specifies the method of instrumented indentation test for determination of hardness and other materials parameters for the following three ranges: macro range: 2 N ≤ F ≤ 30 kN; micro range: 2 N > F; h > 0,2 µm; nano range: h ≤ 0,2 µm. For the nano range, the mechanical deformation strongly depends on the real shape of indenter tip and the calculated material parameters are significantly influenced by the contact area function of the indenter used in the testing machine. Therefore, careful calibration of both instrument and indenter shape is required in order to achieve an acceptable reproducibility of the materials parameters determined with different machines. The macro and micro ranges are distinguished by the test forces in relation to the indentation depth. Attention is drawn to the fact that the micro range has an upper limit given by the test force (2 N) and a lower limit given by the indentation depth of 0,2 µm. The determination of hardness and other material parameters is given in the normative Annex A. At high contact pressures, damage to the indenter is possible. For test pieces with very high hardness and modulus of elasticity, permanent indenter deformation can occur and can be detected using suitable reference materials. Indentations that result in damage or permanent deformation of the indenter are excluded from the scope of this test method. This test method can also be applied to thin metallic and non-metallic coatings and non-metallic materials. In this case, it is recommended that the specifications in the relevant standards be taken into account (see also 7.3 and ISO 14577-4). The analysis methods of this standard assume that materials behave like ideal materials. Any deviation (internal stress, pile-up, sink-in, densification, phase transitions, cracks) will result in additional uncertainties. This becomes especially important if comparisons shall be done to material parameters, obtained with other methods.
- Status
- Published
- Publication Date
- 15-Jun-2026
- Technical Committee
- ISO/TC 164/SC 3 - Hardness testing
- Current Stage
- 6060 - International Standard published - 60 Publication
- Start Date
- 16-Jun-2026
- Due Date
- 20-Mar-2026
- Completion Date
- 20-Mar-2026
Buy Documents
ISO 14577-1:2026 - Metallic materials — Instrumented indentation test for hardness and materials parameters — Part 1: Test method
ISO 14577-1:2026 - Matériaux métalliques — Essai de pénétration instrumenté pour la détermination de la dureté et de paramètres des matériaux — Partie 1: Méthode d'essai
ISO 14577-1:2026 is an ISO International Standard for instrumented indentation testing of metallic materials. It specifies the test method used to determine indentation hardness and other materials parameters, and it is written for laboratories, engineers, and quality teams that need force-depth results they can compare across machines. The same method can also be applied to thin metallic and non-metallic coatings and other non-metallic materials when the related standards are taken into account.
What does ISO 14577-1:2026 specify?
ISO 14577-1:2026 specifies the method for instrumented indentation tests in three ranges: macro, micro, and nano. It defines how the test is carried out, how the data are recorded and analysed, and what must be reported so the results are traceable and comparable.
The document is organized into:
- Clause 1 Scope
- Clause 2 Normative references
- Clause 3 Terms and definitions
- Clause 4 Symbols and designations
- Clause 5 Principle
- Clause 6 Testing machine
- Clause 7 Test piece
- Clause 8 Procedure
- Clause 9 Uncertainty of the results
- Clause 10 Test report
- Annexes A to I covering calculation methods, control modes, calibration, uncertainty, and corrections
| Annex | What it covers |
|---|---|
| A | Materials parameters determined from the force/indentation depth data set |
| B | Types of control used for the indentation process |
| C | Machine compliance and indenter area function |
| D | Notes on diamond indenters |
| E | Influence of test piece surface roughness on the accuracy of the results |
| F | Correlation of indentation hardness H to Vickers hardness |
| G | Determination of drift and minimizing creep influence |
| H | Estimation of uncertainty of calculated hardness and materials parameters |
| I | Calculation of radial displacement correction |
The scope also makes two practical limits clear. First, indentations that damage the indenter or cause permanent indenter deformation are outside the method. Second, the analysis assumes ideal material behavior, so pile-up, sink-in, densification, phase transitions, cracking, and internal stress add uncertainty and matter most when comparing results with other methods.
What are the key requirements of ISO 14577-1:2026?
ISO 14577-1:2026 is not just a calculation standard - it also sets the test setup, specimen conditions, measurement sequence, and reporting content needed for usable results. The most important requirements are below.
Test machine and indenter
The testing machine must be able to apply predetermined force or displacement, record force, indentation depth, and time through the full cycle, compensate for machine compliance, and use the correct indenter area function. It must also comply with ISO 14577-2:2026, which is the companion standard for verification and calibration.
The indenter must be harder than the test piece and must not permanently deform or be damaged during the test. Diamond is preferred, but other materials such as sapphire may be used if they meet the mechanical requirements. The standard discusses Vickers, modified Berkovich, ball, and spherical tipped conical indenters, and it allows other geometries if the results are interpreted with care.
Test piece surface, thickness, and spacing
The test surface must be suitable for the indentation range and free from fluids or lubricants unless those are essential and reported. Cleaning should be limited to gentle methods, because aggressive cleaning can damage the surface or coating.
Surface finish matters because roughness changes the contact area at shallow depths. The surface must also be normal to the indentation direction within 1°, and the effect of tilt belongs in the uncertainty budget. The specimen must be thick enough, or the indentation shallow enough, that support effects do not distort the result - for hardness and modulus, the thickness rule is based on 10 times the indentation depth or 3 times the indentation diameter, whichever is greater.
Indentations must also be kept away from edges, interfaces, and other indentations. This matters in practice because nearby free surfaces or previous indents can make hardness and modulus appear higher or lower than they really are.
Procedure, drift, and loading profile
The test temperature must be recorded, and the test should be run within ±10 °C of the instrument calibration temperature. The standard recommends controlled laboratory conditions and stable temperature over the full cycle. If thermal drift affects the result, the displacement data must be corrected and the drift uncertainty reported.
Each test needs its own zero point for the force-depth curve. ISO 14577-1:2026 allows two main approaches: a fitted extrapolation method or a touch-point method based on the first increase in force or stiffness. The chosen method and its uncertainty must be reported.
The test cycle may be force-controlled or displacement-controlled, and the full profile must be documented, including hold periods and logging frequency. The standard also notes that approach speed must be low enough to avoid changing the surface response at contact, and that shock, vibration, and air movement should be controlled because they affect small-depth measurements.
Data reduction, uncertainty, and reporting
Annex A gives the formulas for indentation hardness H, Martens hardness HM, indentation modulus E, creep, relaxation, and elastic work ratio. H is based on the projected contact area under load, while E is derived from the unloading compliance and the test piece Poisson’s ratio. Annex I then corrects for radial displacement, which becomes important when comparing materials with different elastic behavior.
Clause 9 requires uncertainty evaluation in line with ISO/IEC Guide 98-3. The main contributors include zero-point assignment, force and displacement measurement, curve fitting, thermal drift, surface roughness, machine compliance, indenter area function, calibration drift, and surface tilt.
The test report must identify the standard used, the test piece, the indenter and area function, the full cycle profile, the result and expanded uncertainty, the zero-point method, any non-standard operations, the test temperature, date and time, and the analysis methods.
What terms does ISO 14577-1:2026 define?
ISO 14577-1:2026 uses the following key symbols and designations in its calculations.
- H - Indentation hardness, a measure based on the maximum force and the projected contact area under load.
- HM - Martens hardness, measured under applied test force from the force-depth curve.
- E - Indentation modulus, derived from the unloading compliance and the material’s Poisson’s ratio.
- F - Test force, the applied load during the indentation cycle.
- h - Indentation depth, the penetration depth of the indenter into the test piece.
- C - Indentation creep, the relative change in depth while the force is held constant.
- R - Indentation relaxation, the relative change in force while the indentation depth is held constant.
Who uses ISO 14577-1:2026?
ISO 14577-1:2026 is used by materials testing laboratories, hardness testing specialists, and research teams that need force-depth indentation data. It is also used by manufacturers and quality managers who specify or verify hardness and related material parameters for metals, coatings, and other materials.
In practice, users apply it to:
- set up and run instrumented indentation tests
- calibrate and check machines and indenters
- compare hardness, modulus, creep, and relaxation results
- report results with an uncertainty statement
- support product qualification, incoming inspection, and process control
What changed in ISO 14577-1:2026 from the previous edition?
ISO 14577-1:2026 is the third edition and cancels and replaces ISO 14577-1:2015. The foreword lists these technical changes:
- better specification of the approach speed of the tip
- addition of a loading method with constant strain rate
- change in the order of hardness definitions, with H before HM
- better proposals for cleaning the tip
- differentiation between contact area under load and in the unloaded state
- complete reformulation of normative Annex I for radial displacement correction
Which standards are used with ISO 14577-1:2026?
- ISO 14577-2:2026 - Specifies verification and calibration of the testing machine, and the document relies on it for machine performance, compliance, and indenter verification.
- ISO/IEC Guide 98-3:2008 - Provides the uncertainty framework used in Clause 9 and Annex H.
- ISO 14577-4 - Provides the test method for metallic and non-metallic coatings, which the scope points to for thin coatings and related cases.
- ISO 14577-3 - Covers calibration of reference blocks in the ISO 14577 series, and is listed in the bibliography for supporting work.
- ISO 4287 - Supplies the surface roughness term Ra used in Annex E.
- ISO 6507-1 - Provides the conventional Vickers hardness reference used when Annex F relates H to Vickers hardness.
What does the ISO 14577-1:2026 document contain?
ISO 14577-1:2026 contains the full test method, the symbol set, the machine and specimen requirements, the procedure, the uncertainty approach, and the reporting rules. It also includes figures for the force-depth cycle, indentation geometry, drift handling, and control modes.
The annexes provide the calculation tools that support the method in practice. Annex A covers the formulas for H, HM, E, creep, relaxation, and indentation work; Annex C covers machine compliance and indenter area function; Annex H gives the uncertainty workflow; and Annex I provides the radial displacement correction used in hardness and modulus calculations.
Relations
- Effective Date
- 09-Sep-2026
- Effective Date
- 12-Feb-2026
- Effective Date
- 25-Jun-2022
Buy Documents
ISO 14577-1:2026 - Metallic materials — Instrumented indentation test for hardness and materials parameters — Part 1: Test method
ISO 14577-1:2026 - Matériaux métalliques — Essai de pénétration instrumenté pour la détermination de la dureté et de paramètres des matériaux — Partie 1: Méthode d'essai
Get Certified
Connect with accredited certification bodies for this standard

Element Materials Technology
Materials testing and product certification.

Inštitut za kovinske materiale in tehnologije
Institute of Metals and Technology. Materials testing, metallurgical analysis, NDT.
Sponsored listings
Frequently Asked Questions
ISO 14577-1:2026 is a standard published by the International Organization for Standardization (ISO). Its full title is "Metallic materials — Instrumented indentation test for hardness and materials parameters — Part 1: Test method". This standard covers: This document specifies the method of instrumented indentation test for determination of hardness and other materials parameters for the following three ranges: macro range: 2 N ≤ F ≤ 30 kN; micro range: 2 N > F; h > 0,2 µm; nano range: h ≤ 0,2 µm. For the nano range, the mechanical deformation strongly depends on the real shape of indenter tip and the calculated material parameters are significantly influenced by the contact area function of the indenter used in the testing machine. Therefore, careful calibration of both instrument and indenter shape is required in order to achieve an acceptable reproducibility of the materials parameters determined with different machines. The macro and micro ranges are distinguished by the test forces in relation to the indentation depth. Attention is drawn to the fact that the micro range has an upper limit given by the test force (2 N) and a lower limit given by the indentation depth of 0,2 µm. The determination of hardness and other material parameters is given in the normative Annex A. At high contact pressures, damage to the indenter is possible. For test pieces with very high hardness and modulus of elasticity, permanent indenter deformation can occur and can be detected using suitable reference materials. Indentations that result in damage or permanent deformation of the indenter are excluded from the scope of this test method. This test method can also be applied to thin metallic and non-metallic coatings and non-metallic materials. In this case, it is recommended that the specifications in the relevant standards be taken into account (see also 7.3 and ISO 14577-4). The analysis methods of this standard assume that materials behave like ideal materials. Any deviation (internal stress, pile-up, sink-in, densification, phase transitions, cracks) will result in additional uncertainties. This becomes especially important if comparisons shall be done to material parameters, obtained with other methods.
This document specifies the method of instrumented indentation test for determination of hardness and other materials parameters for the following three ranges: macro range: 2 N ≤ F ≤ 30 kN; micro range: 2 N > F; h > 0,2 µm; nano range: h ≤ 0,2 µm. For the nano range, the mechanical deformation strongly depends on the real shape of indenter tip and the calculated material parameters are significantly influenced by the contact area function of the indenter used in the testing machine. Therefore, careful calibration of both instrument and indenter shape is required in order to achieve an acceptable reproducibility of the materials parameters determined with different machines. The macro and micro ranges are distinguished by the test forces in relation to the indentation depth. Attention is drawn to the fact that the micro range has an upper limit given by the test force (2 N) and a lower limit given by the indentation depth of 0,2 µm. The determination of hardness and other material parameters is given in the normative Annex A. At high contact pressures, damage to the indenter is possible. For test pieces with very high hardness and modulus of elasticity, permanent indenter deformation can occur and can be detected using suitable reference materials. Indentations that result in damage or permanent deformation of the indenter are excluded from the scope of this test method. This test method can also be applied to thin metallic and non-metallic coatings and non-metallic materials. In this case, it is recommended that the specifications in the relevant standards be taken into account (see also 7.3 and ISO 14577-4). The analysis methods of this standard assume that materials behave like ideal materials. Any deviation (internal stress, pile-up, sink-in, densification, phase transitions, cracks) will result in additional uncertainties. This becomes especially important if comparisons shall be done to material parameters, obtained with other methods.
ISO 14577-1:2026 is classified under the following ICS (International Classification for Standards) categories: 77.040.10 - Mechanical testing of metals. The ICS classification helps identify the subject area and facilitates finding related standards.
ISO 14577-1:2026 has the following relationships with other standards: It is inter standard links to EN ISO 14577-2:2026, EN ISO 14577-1:2026, ISO 14577-1:2015. Understanding these relationships helps ensure you are using the most current and applicable version of the standard.
ISO 14577-1:2026 is available in PDF format for immediate download after purchase. The document can be added to your cart and obtained through the secure checkout process. Digital delivery ensures instant access to the complete standard document.
Standards Content (Sample)
Contents
- Introduction
- 1 Scope
- 2 Normative references
- 3 Terms and definitions
- 4 Symbols and designations
- 5 Principle
- 6 Testing machine
- 7 Test piece
- 8 Procedure
- 9 Uncertainty of the results
- 10 Test report
- Annex A
- Annex B
- Annex C
- Annex D
- Annex E
- Annex F
- Annex G
- 2 E dt
- Annex H
- Annex I
- 2 E E E
- Bibliography
Introduction
Hardness has typically been defined as the resistance of a material to permanent penetration by another harder material. The results obtained when performing Rockwell, Vickers, and Brinell tests are determined after the test force has been removed. Therefore, the effect of elastic deformation under the indenter has been ignored.
ISO 14577 (all parts) has been prepared to enable the user to evaluate the indentation of materials by considering both the force and displacement during plastic and elastic deformation. By monitoring the complete cycle of increasing and removal of the test force, hardness values equivalent to traditional hardness values can be determined. More significantly, additional properties of the material, such as its indentation modulus and elasto-plastic hardness, can also be determined. All these values can be calculated without the need to measure the indent optically. Furthermore, by a variety of techniques, the instrumented indentation test allows to record hardness and modulus depth profiles within a, probably complex, indentation cycle. Although the indentation modulus (E ) value obtained in this test method is not directly equivalent to IT Young’s modulus or the orientation specific elastic modulus of the material indented, E is, however, IT equivalent to the isotropic Hill average of the elastic plane strain modulus of the material when there is no pile up and no residual stress.
ISO 14577 (all parts) has been written to allow a wide variety of post-test data analysis. Part 1 of ISO 14577 specifies the method of indentation test for determination of instrumented indentation hardness and material properties.
International Standard ISO 14577-1:2026(en) Metallic materials — Instrumented indentation test for hardness and materials parameters — Part 1:
Test method
1 Scope
This document specifies the method of instrumented indentation test for determination of hardness and other materials parameters for the following three ranges:
- macro range: 2 N ≤ F ≤ 30 kN;
- micro range: 2 N > F; h > 0,2 µm;
- nano range: h ≤ 0,2 µm.
For the nano range, the mechanical deformation strongly depends on the real shape of indenter tip and the calculated material parameters are significantly influenced by the contact area function of the indenter used in the testing machine. Therefore, careful calibration of both instrument and indenter shape is required in order to achieve an acceptable reproducibility of the materials parameters determined with different machines.
The macro and micro ranges are distinguished by the test forces in relation to the indentation depth. Attention is drawn to the fact that the micro range has an upper limit given by the test force (2 N) and a lower limit given by the indentation depth of 0,2 µm.
The determination of hardness and other material parameters is given in the normative Annex A. At high contact pressures, damage to the indenter is possible. For test pieces with very high hardness and modulus of elasticity, permanent indenter deformation can occur and can be detected using suitable reference materials. Indentations that result in damage or permanent deformation of the indenter are excluded from the scope of this test method.
This test method can also be applied to thin metallic and non-metallic coatings and non-metallic materials. In this case, it is recommended that the specifications in the relevant standards be taken into account (see also 7.3 and ISO 14577-4).
The analysis methods of this standard assume that materials behave like ideal materials. Any deviation (internal stress, pile-up, sink-in, densification, phase transitions, cracks) will result in additional uncertainties. This becomes especially important if comparisons shall be done to material parameters, obtained with other methods.
2 Normative references
The following documents, in whole or in part, are normatively referenced in this document and are indispensable for its application. For dated references, only the edition cited applies. For undated references, the latest edition of the referenced document (including any amendments) applies. ISO 14577-2:2026, Metallic materials — Instrumented indentation test for hardness and materials parameters - Part 2: Verification and calibration of testing machines
ISO 14577-1:2026(en) ISO/IEC Guide 98-3:2008, Uncertainty of measurement — Part 3: Guide to the expression of uncertainty in me a s ur ement (GUM: 1995)
3 Terms and definitions
No terms and definitions are listed in this document.
ISO and IEC maintain terminology databases for use in standardization at the following addresses:
- ISO Online browsing platform: available at https:// www .iso .org/ obp
- IEC Electropedia: available at https:// www .electropedia .org/
4 Symbols and designations
For the purposes of this document, the symbols and designations in Table 1 shall be applied (see also Figure 1 and Figure 2).
Table 1 — Symbols and designations Symbol Designation Unit
A (h ) Projected area of contact under load of the indenter at distance h from the tip mm p c c
Projected area of contact in unloaded state of the indenter at distance h from the mm
A (h ) p,UL c tip
A (h) Surface area of the indenter at distance h from the tip in unloaded state mm s C Indentation creep % IT Total measured compliance of the contact (dh/dF tangent to the force removal nm/mN C T curve at maximum test force) C Machine compliance nm/mN F C Compliance of the contact after correction for machine compliance nm/mN S E Indentation modulus of the test piece GPa IT Reduced plane strain modulus of the contact (combination of test piece and in- GPa E r denter plane strain moduli) F Test force N F Maximum test force N max h Indentation depth under applied test force mm h Contact depth of the indenter with the test piece at F mm c max h Maximum indentation depth at F mm max max h Permanent indentation depth after removal of the test force mm p Point of intersection of the tangent c to curve b at F with the indentation mm max h r depth-axis as identified on Figure 1 H Indentation hardness GPa IT HM Martens hardness GPa Martens hardness, determined from the slope of the increasing GPa HM s force/indentation depth curve GPa HM Martens hardness, determined from the first derivative of h vs F diff ν Poisson’s ratio of the test piece s r Radius of spherical indenter mm R Indentation relaxation % IT NOTE 1 To avoid very long numbers, the use of multiples or sub-multiples of the units can be used. 2 2 NOTE 2 The continued use of the unit N/mm is allowed. 1 MPa = 1 N/mm .
ISO 14577-1:2026(en) TTabablele 1 1 ((ccoonnttiinnueuedd)) Symbol Designation Unit W Elastic reverse deformation work of indentation N⋅m elast W Total mechanical work of indentation N⋅m total Cone semi-angle or angle of facet to the indentation axis for pyramidal ° α indenters Maximum angle between the contact surface and the indenter for calculation of ° θ radial displacement η Ratio W /W % IT elast total NOTE 1 To avoid very long numbers, the use of multiples or sub-multiples of the units can be used. 2 2 NOTE 2 The continued use of the unit N/mm is allowed. 1 MPa = 1 N/mm .
a Application of the test force.
b Removal of the test force.
Tangent to curve b at F .
max Figure 1 — Schematic representation of the test procedure
ISO 14577-1:2026(en) Key a Indenter.
b Surface of residual plastic indentation in a test piece that has a “perfectly plastic” response.
Surface of test piece at maximum indentation depth and test force. θ maximum angle between the test piece surface and the indenter Figure 2 — Schematic representation of the cross section of indentation in the case of material “sink-in”
5 Principle
Continuous recording of the force and the depth of indentation permits the determination of hardness and material properties (see Figure 1 and Figure 2). The measured values of hardness and other material parameters shall be determined in accordance with Annex A. An indenter consisting of a material harder than the material under test shall be used (i.e. the indenter shall not permanently deform and shall not be damaged as a result of indentation). For hardness testing the following shapes and materials can be used:
a) indenter shaped as an orthogonal pyramid with a square base and with an angle α = 68° between the axis of the diamond pyramid and one of the faces (Vickers pyramid; see Figure A.1); b) pyramid with triangular base (e.g. modified Berkovich pyramid with an angle α = 65,27° between the axis of the diamond pyramid and one of the faces; see Figure A.1); c) ball indenter (especially for the determination of the elastic behaviour of materials); d) spherical tipped conical indenter.
This document does not preclude the use of other indenter geometries; however, care should be taken when interpreting the results obtained with such indenters. Diamond is the preferred material but other materials like sapphire may also be used for example to avoid chemical reaction between the indenter and the test piece, provided the above mechanical requirements of the indenter are met. For indentation modulus testing, the indenter geometries for hardness testing are strongly recommended but, in principle, any geometry indenter may be used provided that the area function is known and the area function is monotonically increasing with indentation depth.
NOTE Due to the crystal structure of diamond, indenters that are intended to be spherical are often polyhedrons and do not have an ideal spherical shape.
The test procedure can either be force-controlled or displacement-controlled. The test force, F, the corresponding indentation depth, h, and time are recorded during the whole test procedure. The result of the test is the data set of the test force and the relevant indentation depths as a function of time (see Figure 1 and Annex B).
For a reproducible determination of the force and corresponding indentation depth, the zero point for the force/indentation depth measurement shall be assigned individually for each test (see 7.3).
ISO 14577-1:2026(en) Where time-dependent effects are being measured - using the force-controlled method, the test force is kept constant over a specified period and the change of the indentation depth is measured as a function of the holding time of the test force (see Figures A.3 and B.1), and - using the indentation depth-controlled method, the indentation depth is kept constant over a specified period and the change of the test force is measured as a function of the holding time of the indentation depth (see Figures A.4 and B.2).
The two kinds of control mentioned give essentially different results in the segment b of the curves in Figure B.1 a) and Figure B.2 b) or in Figure B.1 b) and Figure B.2 a).
6 Testing machine
6.1 The testing machine shall have the capability of applying predetermined test forces or displacements within the required scope and shall fulfil the requirements of ISO 14577-2. 6.2 The testing machine shall have the capability of measuring and reporting applied force, indentation displacement and time throughout the testing cycle.
6.3 The testing machine shall have the capability of compensating for the machine compliance and of utilizing the appropriate indenter area function according to Annex C and ISO 14577-2:2026, 5.5 and 5.6. 6.4 Indenters for use with testing machines can have various shapes, as specified in ISO 14577-2 (for further information on indenters, see Annex D).
6.5 The testing machine shall operate at a temperature within the permissible range specified in 7.1 and shall maintain its calibration within the limits specified in ISO 14577-2:2026, Clause 5.
7 Test piece
7.1 The test shall be carried out on a region of the test surface that allows the determination of the force/ indentation depth curve for the respective indentation range within the required uncertainty. The contact area shall be free of fluids or lubricants except where this is essential for the performance of the test, in which case, this shall be described in detail in the test report. Care shall be taken that extraneous matter (e.g. dust particles) is not incorporated into the contact.
Generally, provided the surface is free from obvious surface contamination, cleaning procedures should be avoided. If cleaning is required, it shall be limited to the following methods to minimize damage:
- application of a dry, oil-free, filtered gas stream;
- application of a subliming particle stream of CO (but keeping the surface temperature above the dew
point); - rinsing with a solvent (which is chemically inert to the test piece) and then setting it to dry. If these methods fail and the surface is sufficiently robust, wipe the surface with a lint-free tissue soaked in solvent to remove trapped dust particles, after which, the surface shall be rinsed in a solvent as above. Ultrasonic methods are known to create or increase damage to surfaces and coatings and should only be used with caution.
Surface finish has a significant influence on the test results that depends upon the relative size of the indentation depth, h, with respect to the arithmetic mean deviation roughness, Ra. The relative size of these parameters shall conform to the limits given in Annex E.
ISO 14577-1:2026(en) The test piece surface shall be normal to the test force direction. The angle difference between test surface normal and indenter axis shall be less than 1°. The effect of surface tilt should be included in the uncertainty calculation.
The sample should be free from magnetism. Test pieces capable of becoming magnetised should be checked for magnetism and demagnetised before testing, if possible. Precautions should be taken to avoid the effect of magnetism on the measuring system.
7.2 If necessary, preparation of the test surface shall be carried out in such a way that any alteration of the surface hardness and/or surface residual stress (e.g. due to heat or cold-working) is minimized. Due to the small indentation depths in the micro and nano range, special precautions shall be taken during the test piece preparation. When polishing is needed, a polishing process that is suitable for the particular materials shall be used.
Electropolishing is a recommended preparation method that can remove a work hardened surface layer. However, care should be taken that the surface roughness does not exceed the limits given in this standard. 7.3 The test piece thickness shall be large enough (or indentation depth small enough) such that the test result is not influenced by the test piece support. For hardness and modulus measurements, the test piece thickness shall be at least 10 times the indentation depth or 3 times the indentation diameter (see 8.7), whichever is greater. For modulus measurements a sample thickness larger than 30 times the indentation depth is recommended. For measurements of thinner samples, it is recommended to follow the analysis described in ISO 14577-4 for coatings.
When testing coatings, the coating thickness should be considered as the test piece thickness. For testing thin samples or coatings, see ISO 14577-4 for better testing procedures. NOTE The above are empirically based limits based on hardness testing. The effect of test piece thickness on the elastic modulus result is not the same as the effect on the hardness result. The exact limits of influence of support on test piece depend on the geometry of the indenter used and the materials properties of the test piece and support.
8 Procedure
8.1 The temperature of the test shall be recorded. Tests shall be performed within ±10 °C of the temperature of the instrument calibration.
The temperature stability during a test is more important than the actual test temperature. Any calibration correction applied shall be reported along with the additional calibration uncertainty. It is recommended that tests, particularly in the nano and micro ranges, be performed in controlled conditions, in the range (23 ± 5) °C and (45 ± 10) % relative humidity.
The individual tests, however, shall be carried out at stable temperature conditions because of the requirement of high depth measuring accuracy. This means that:
- the test pieces shall have reached the ambient temperature before testing,
- the testing machine shall have reached a stable working temperature (operating manual should be consulted),
- the ambient, instrument, and test temperature shall be within the range for which the machine calibration is valid, and
- other external influences causing temperature changes during individual test have been controlled. To minimize thermally induced displacement drift, the temperature of the testing machine shall be adequately maintained over the time period of one testing cycle, or a displacement drift shall be measured and corrected. A decision tree to assist in estimating the drift during the experiment is shown in Figure 3. If the drift rate is significant, the displacement data shall be corrected by measuring the drift rate during a hold at an applied force as close to zero force as is practicable or during a hold at a suitable place in the
ISO 14577-1:2026(en) force removal curve in accordance with Annex G and ISO 14577-2:2026, 5.3.3). In all cases where the drift rate would influence the maximum indentation depth by more than 1 % within the total indentation cycle time, the drift rate shall be corrected (see tolerances in ISO 14577-2:2026, Table 2 and 5.3.3). If a contact in the fully elastic regime can be obtained, a hold at initial contact is preferred. In this way, material influences (creep, visco-plasticity, cracking) can be minimized. When the measurement is significantly longer than the hold period for thermal drift measurement it is recommended to measure the thermal drift before and after the experiment and to correct the displacement using the average of the two drift rates. The difference between the two drift rates is an estimate of the drift rate uncertainty. The uncertainty due to the drift, or in the drift correction used, shall be reported.
To determine the drift of surface referenced instruments, contact between the reference indenter and the sample surface shall be elastic. This may be determined by calculation. NOTE The significance of a particular drift rate upon the measurement depends upon the range of the indentation and the type of application.
Figure 3 — Decision tree to assist in estimating thermal drift using a constant force hold period 8.2 The test piece shall be firmly supported such that there is no significant change in the testing machine compliance. The test piece shall either be placed on a support that is rigid in the direction of indentation or be fixed in a suitable test piece holder. The contact surfaces between test piece support and test piece holder shall be free from extraneous matter, which can increase the compliance (reduce the stiffness) of the test piece support.
If the sample is supported by materials or mounting methods other than those used when determining the machine compliance, then the different elastic response of these materials and mounting methods can cause additional compliance. A certified reference material, mounted in the same way as the sample, should be
...
Contents
- Introduction
- 1 Domaine d'application
- 2 Références normatives
- 3 Termes et définitions
- 4 Symboles et désignations
- 5 Principe
- 6 Machine d'essai
- 7 Éprouvette
- 7.3 L'épaisseur de l'éprouvette doit être suffisamment grande (ou la profondeur de pénétration
- 8 Mode opératoire
- 8.3 Le point zéro pour le mesurage de la courbe force/profondeur de pénétration doit être fixé
- 9 Incertitude des résultats
- 10 Rapport d’essai
- Annexe A
- Annexe B
- Annexe C
- Annexe D
- Annexe E
- Annexe F
- Annexe G
- 2 E dt
- Annexe H
- Annexe I
- 2 E E E
- Bibliographie
Introduction
La dureté a été typiquement définie comme la résistance d'un matériau à la pénétration rémanente par un autre matériau plus dur. Les résultats obtenus lors d'essais Rockwell, Vickers et Brinell sont déterminés après retrait de la force d'essai. En conséquence, l'effet de la déformation élastique sous le pénétrateur a été ignoré.
L’ISO 14577 (toutes les parties) a été préparée pour permettre à l'utilisateur d'évaluer la pénétration des matériaux en prenant en compte la force et le déplacement pendant les déformations plastique et élastique. En suivant le cycle complet d'augmentation et de retrait de la force d'essai, il est possible de déterminer des valeurs de dureté équivalentes aux valeurs traditionnelles de dureté. Plus important encore, il est également possible de déterminer des caractéristiques complémentaires du matériau telles que son module de pénétration et sa dureté élasto-plastique. Toutes ces valeurs peuvent être calculées sans qu'il y ait à mesurer l'empreinte par des moyens optiques. De plus, l’essai de pénétration instrumenté permet d’enregistrer des profils de dureté et de module en fonction de la profondeur, par une variété de techniques, lors d’un cycle de pénétration probablement complexe.
Bien que la valeur du module de pénétration (E ) obtenue dans la présente méthode d’essai ne soit pas IT directement équivalente au module de Young ou au module élastique spécifique d’orientation du matériau pénétré, l’E est cependant équivalent à la moyenne de Hill isotrope du module de déformation élastique du IT matériau lorsqu’il n’y a pas d’empilement ni de contrainte résiduelle. L'ISO 14577 (toutes les parties) a été rédigée pour permettre une grande diversité d'analyses des données après essai.
La Partie 1 de l’ISO 14577 spécifie la méthode d’essai par indentation pour la détermination de la dureté par indentation instrumentée et des propriétés des matériaux.
Norme internationale ISO 14577-1:2026(fr) Matériaux métalliques — Essai de pénétration instrumenté pour la détermination de la dureté et de paramètres des matériaux — Partie 1:
Méthode d'essai
1 Domaine d'application
Le présent document spécifie la méthode d'essai de pénétration instrumenté pour la détermination de la dureté et d'autres paramètres des matériaux pour les trois plages suivantes:
- macro-intervalle: 2 N ≤ F ≤ 30 kN;
- micro-intervalle: 2 N > F; h > 0,2 µm;
- nano-intervalle: h ≤ 0,2 µm.
Pour le nano-intervalle, la déformation mécanique dépend fortement de la forme réelle de la pointe du pénétrateur, et les paramètres des matériaux calculés sont influencés de manière significative par la fonction de l'aire de contact du pénétrateur utilisé sur la machine d'essai. En conséquence, un étalonnage soigné de l'instrument et de la forme du pénétrateur est nécessaire pour obtenir une reproductibilité acceptable des paramètres des matériaux déterminés avec différentes machines. Les macro et micro-intervalles se distinguent par les forces d'essai en relation avec la profondeur d'empreinte. L'attention est attirée sur le fait que le micro-intervalle a une limite supérieure donnée par la force d'essai (2 N) et une limite inférieure donnée par la profondeur d'empreinte de 0,2 µm. La détermination de la dureté et d'autres paramètres des matériaux est donnée dans l'Annexe A normative. L'endommagement du pénétrateur est possible pour les pressions de contact élevées. Pour les éprouvettes à dureté et module d'élasticité élevés, une déformation permanente du pénétrateur peut se produire et être détectée à l’aide des matériaux de référence appropriés. Les pénétrations entraînant des dommages ou une déformation permanente du pénétrateur sont exclues du domaine d’application de la présente méthode d’essai.
La présente méthode d'essai est également applicable à des revêtements métalliques et non métalliques minces et à des matériaux non métalliques. Dans ce cas, il est recommandé de prendre en compte les spécifications données dans les normes applicables (voir également 7.3 et l’ISO 14577-4). Les méthodes d’analyse de la présente norme supposent que les matériaux se comportent comme des matériaux idéaux. Toute déviation (contrainte interne, accumulation, affaissement, densification, transitions de phase, fissures) entraînera des incertitudes supplémentaires. Cela devient particulièrement important si des comparaisons doivent être faites avec des paramètres de matériaux obtenus par d’autres méthodes.
2 Références normatives
Les documents suivants, en tout ou partie, sont référencés de manière normative dans le présent document et sont indispensables à son application. Pour les références datées, seule l'édition citée s'applique. Pour les références non datées, la dernière édition de la publication à laquelle il est fait référence s'applique (y compris tous les amendements).
ISO 14577-1:2026(fr) ISO 14577-2:2026, Matériaux métalliques — Essai de pénétration instrumenté pour la détermination de la dureté et de paramètres des matériaux — Partie 2: Vérification et étalonnage des machines d’essai Guide ISO/IEC 98-3:2008, Incertitude de mesures — Partie 3: Guide pour l’expression de l’incertitude de mesure (GUM: 1995)
3 Termes et définitions
Aucun terme n'est défini dans le présent document.
L'ISO et l'IEC tiennent à jour des bases de données terminologiques destinées à être utilisées en normalisation, consultables aux adresses suivantes:
- ISO Online browsing platform: disponible à l'adresse https:// www .iso .org/ obp
- IEC Electropedia: disponible à l'adresse https:// www .electropedia .org/
4 Symboles et désignations
Pour les besoins du présent document, les symboles et les désignations du Tableau 1 doivent être appliqués (voir également Figure 1 et Figure 2).
Tableau 1 — Symboles et désignations Symbole Désignation Unité
A (h ) Aire de contact projetée du pénétrateur à la distance h de la pointe mm p c c
Aire de contact projetée à l’état non chargé du pénétrateur à la distance h de la mm
A (h ) p,UL c pointe.
A (h) Aire de la surface du pénétrateur à la distance h de la pointe mm s C Fluage de pénétration % IT Compliance de contact totale mesurée (dh/dF tangente à la courbe de retrait de nm/mN C T la force au point correspondant à la force d’essai maximale durant l’essai) C Compliance de la machine nm/mN F C Compliance de contact après correction de la compliance de la machine nm/mN S E Module de pénétration de l’éprouvette GPa IT Module de contact en déformation plane réduite (combinaison des modules en GPa E r déformation plane de l’éprouvette et du pénétrateur) F Force d'essai N F Force maximale d'essai N max h Profondeur de pénétration sous la force d'essai appliquée mm h Profondeur du contact du pénétrateur avec l'éprouvette à F mm c max h Profondeur de pénétration maximale à F mm max max h Profondeur de pénétration rémanente après retrait de la force d'essai mm p Point d'intersection de la tangente c à la courbe b à F avec l'axe profondeur mm max h r de pénétration, comme identifié à la Figure 1 H Dureté de pénétration GPa IT HM Dureté Martens GPa Dureté Martens, déterminée à partir de la pente de la courbe force croissante/ GPa HM s profondeur de pénétration Dureté Martens, déterminée à partir de la dérivée première de h en fonction de GPa HM diff F NOTE 1 De manière à éviter des nombres très longs, l'utilisation de multiples ou sous-multiples des unités peut être utilisée. 2 2 NOTE 2 L’utilisation du N/mm est encore autorisée. 1 MPa = 1 N/mm .
ISO 14577-1:2026(fr) TTabableleaauu 1 1 ((ssuuiitte)e) Symbole Désignation Unité ν Coefficient de poisson de l’éprouvette s r Rayon du pénétrateur sphérique mm R Relaxation de pénétration % IT Travail correspondant à la déformation due au retour élastique lors de la péné- N⋅m W elast tration W Travail mécanique total N⋅m total Demi-angle du cône ou angle de facette par rapport à l’axe du pénétrateur pour ° α les pénétrateurs pyramidaux Angle maximal entre la surface de contact et le pénétrateur pour le calcul du ° θ déplacement radial η Rapport W /W % IT élast total NOTE 1 De manière à éviter des nombres très longs, l'utilisation de multiples ou sous-multiples des unités peut être utilisée. 2 2 NOTE 2 L’utilisation du N/mm est encore autorisée. 1 MPa = 1 N/mm .
a Application de la force d'essai.
b Retrait de la force d'essai.
Tangente à la courbe b à F .
max Figure 1 — Représentation schématique du mode opératoire d'essai
ISO 14577-1:2026(fr) Légende a Pénétrateur.
b Surface de la pénétration plastique résiduelle dans l'éprouvette.
Surface de l'éprouvette pour les profondeurs de pénétration et force d'essai maximales. θ angle maximal entre la surface de contact de l’échantillon et le pénétrateur Figure 2 — Représentation schématique de la coupe transversale de l'empreinte dans le cas d’un enfoncement du matériau
5 Principe
L’enregistrement continu de la force et de la profondeur de pénétration permet la détermination de la dureté et des caractéristiques de matériau (voir Figure 1 et Figure 2). Les valeurs mesurées de dureté et des autres paramètres de matériau doivent être déterminées compliance à l’Annexe A. Un pénétrateur constitué d'un matériau plus dur que le matériau soumis à l'essai doit être utilisé (c’est-à-dire que le pénétrateur ne doit pas être déformé en permanence et ne doit pas être endommagé par suite d’une pénétration). Pour les essais de dureté les formes et les matériaux suivants peuvent être utilisés:
a) pénétrateur en forme de pyramide droite à base carrée avec un angle α = 68° entre l’axe de la pyramide en diamant et l’une des faces (pyramide Vickers, voir Figure A.1); b) pyramide à base triangulaire (par exemple pyramide Berkovich modifiée avec un angle α = 65,27° entre l’axe de la pyramide en diamant et l’une des faces; voir Figure A.1); c) pénétrateur à bille (spécialement pour la détermination du comportement élastique des matériaux); d) pénétrateur à extrémité sphérique.
Le présent document n'exclut pas l'utilisation d'autres géométries de pénétrateur; toutefois, il convient de veiller à interpréter avec prudence les résultats obtenus à l'aide de tels pénétrateurs. Le diamant est le matériau préféré, mais d’autres matériaux comme le saphir peuvent également être utilisés, par exemple pour éviter une réaction chimique entre le pénétrateur et l’éprouvette, à condition que les exigences mécaniques susmentionnées concernant le pénétrateur soient respectées. Pour les essais de module d'indentation, les géométries d'indenteurs utilisées pour les essais de dureté sont fortement recommandées, mais, en principe, toute géométrie d'indenteur peut être utilisée à condition que la fonction de surface soit connue et qu'elle augmente de manière monotone avec la profondeur d'indentation. NOTE En raison de la structure cristalline du diamant, les pénétrateurs qui sont destinés à être sphériques, sont souvent des polyèdres et n’ont pas une forme sphérique idéale. Le mode opératoire d'essai peut être soit à force contrôlée, soit à déplacement contrôlé. La force d'essai, F, la profondeur de pénétration correspondante, h, et le temps sont enregistrés pendant toute la durée de l'essai. L'ensemble des données relatives à la force d'essai et à la profondeur de pénétration correspondante en fonction du temps constitue le résultat de l'essai (voir Figure 1 et Annexe B).
ISO 14577-1:2026(fr) Pour que la détermination de la force et de la profondeur de pénétration correspondante soit reproductible, le point zéro doit être fixé pour le mesurage des forces/profondeurs de pénétration pour chaque essai (voir 7.3).
Lorsque des effets dépendant du temps sont mesurés:
- en utilisant la méthode à force contrôlée, la force d'essai est maintenue constante pendant une durée spécifiée et le changement de la profondeur de pénétration est mesuré en fonction du temps de maintien de la force d'essai (voir Figures A.3 et B.1), et
- en utilisant la méthode à profondeur de pénétration contrôlée, la profondeur de pénétration est maintenue constante pendant un temps spécifié et la modification de la force d'essai est mesurée en fonction du temps de maintien de la profondeur de pénétration (voir Figures A.4 et B.2). Les deux types de contrôles mentionnés donnent des résultats différents, essentiellement pour les zones b des courbes des Figures B.1 a) et B.2 b) ou des Figures B.1 b) et B.2 a).
6 Machine d'essai
6.1 La machine d'essai doit pouvoir appliquer des forces d'essai ou des déplacements prédéterminé(e)s dans l’intervalle requis et doit satisfaire les exigences de l'ISO 14577-2. 6.2 La machine d'essai doit pouvoir mesurer et enregistrer la force appliquée, la pénétration et le temps, pendant tout le cycle d’essai.
6.3 La machine d'essai doit pouvoir compenser la compliance de la machine et utiliser la fonction de l'aire appropriée du pénétrateur selon l’Annexe C et l’ISO 14577-2:2026, 5.5 et 5.6. 6.4 Les pénétrateurs à utiliser avec les machines d'essai peuvent avoir diverses formes, comme spécifié dans l'ISO 14577-2 (pour des informations complémentaires sur les pénétrateurs, voir Annexe D). 6.5 La machine d'essai doit être utilisée à une température comprise dans l'intervalle admissible spécifié en 8.1 et doit conserver son étalonnage dans les limites prescrites dans l’ISO 14577-2:2026, Article 5.
7 Éprouvette
7.1 L'essai doit être réalisé dans une zone de la surface d'essai qui permet la détermination de la courbe force/profondeur de pénétration pour la plage de pénétration correspondante à l'intérieur de l'incertitude requise. La surface de contact doit être exempte de fluides et de lubrifiants, sauf losque cela est essentiel pour la réalisation de l'essai, auquel cas, cela doit être décrit en détail dans le rapport d'essai. Il doit être veillé à ce qu'aucune matière étrangère (par exemple particules de poussières) ne soit incorporée dans la zone de contact.
En général, pour autant que la surface soit exempte d’une contamination évidente de la surface, il convient d’éviter des procédures de nettoyage. Si un nettoyage est requis, il doit être limité à des méthodes qui minimisent les endommagements, par exemple:
- application d’un courant de gaz sec, exempt d’huile et filtré;
- application d’un courant de particules de CO se sublimant (en évitant une température de surface en
dessous du point de rosée); - rincer avec un solvant (qui est chimiquement inerte vis-à-vis de l’éprouvette) puis sécher. Si ces méthodes échouent et que la surface est suffisamment robuste, essuyer la surface avec un tissu non pelucheux imbibé de solvant afin d’enlever les particules de poussière piégées, après quoi, la surface doit être rincée dans un solvant comme décrit précédemment.
ISO 14577-1:2026(fr) Les méthodes par ultrasons sont connues pour créer ou accroître l’endommagement des surfaces et des revêtements et il convient de ne les utiliser qu'avec précaution. Le fini de surface a une influence significative sur les résultats d’essai qui dépend de la taille relative de la profondeur d’indentation, h, par rapport à la rugosité moyenne arithmétique, Ra. La taille relative de ces paramètres doit respecter les limites indiquées dans l’Annexe E. La surface de l’éprouvette doit être perpendiculaire à la direction de la force d’essai. La différence d’angle entre la normale à la surface d’essai et l’axe de l’indenteur doit être inférieure à 1°. Il convient que l’effet de l’inclinaison de la surface soit inclus dans le calcul de l’incertitude. Il convient que l’échantillon soit exempt de magnétisme. Il convient que les éprouvettes susceptibles de devenir magnétiques soient vérifiées quant à la présence de magnétisme et démagnétisées avant l’essai, si possible. Il convient que des précautions soient prises pour éviter l’effet du magnétisme sur le système de mesure.
7.2 Si nécessaire, la préparation de la surface d'essai doit être effectuée de façon que toute altération de la dureté de la surface et/ou toute contrainte résiduelle de surface (par exemple par échauffement ou par écrouissage) soient réduites au minimum.
Compte tenu des faibles profondeurs de pénétration dans les micro et nano-intervalles, des précautions particulières doivent être prises lors de la préparation de l'éprouvette. Lorsqu’un polissage est nécessaire, un procédé de polissage adapté aux matériaux particuliers doit être utilisé. Le polissage électrolytique est une méthode de préparation recommandée qui peut éliminer une couche de surface écrouie. Cependant, il convient de veiller à ce que la rugosité de la surface ne dépasse pas les limites indiquées dans la présente norme.
7.3 L'épaisseur de l'éprouvette doit être suffisamment grande (ou la profondeur de pénétration
suffisamment petite) pour que le résultat d'essai ne soit pas influencé par l'appui de l'éprouvette. Pour les mesurages de dureté et du module, l'épaisseur de l'éprouvette doit être au moins égale à la plus élevée des deux valeurs entre 10 fois la profondeur de pénétration ou à 3 fois le diamètre de l'empreinte (voir 8.7). Pour les mesurages du module, une épaisseur d’échantillon supérieure à 30 fois la profondeur de pénétration est recommandée. Pour les mesurages d’échantillons plus minces, il est recommandé de suivre l’analyse décrite dans l’ISO 14577-4 pour les revêtements.
Lors des essais des revêtements, il convient de considérer que l'épaisseur de l'éprouvette est l'épaisseur du revêtement. Pour soumettre à l’essai des échantillons minces ou des revêtements, voir l’ISO 14577-4 pour réaliser de meilleurs modes opératoires d’essai.
NOTE Ce qui précède correspond à des limites établies de manière empirique basées sur des essais de dureté. L’effet de l’épaisseur de l’éprouvette sur le résultat de module élastique n’est pas le même que l’effet sur le résultat de dureté. Les limites précises de l'influence de l'appui sur l'éprouvette dépendent de la géométrie du pénétrateur utilisé et des caractéristiques des matériaux de l'éprouvette et de l'appui.
8 Mode opératoire
8.1 La température de l'essai doit être enregistrée. Les essais doivent être effectués à ±10 °C de la température d’étalonnage de l’instrument.
La stabilité de la température durant un essai est plus importante que la température d'essai effective. Toute correction de l'étalonnage appliquée doit être indiquée dans le rapport d'essai avec l'incertitude d'étalonnage complémentaire. Il est recommandé que les essais, en particulier ceux dans les nano et micro intervalles, soient réalisés dans des conditions contrôlées dans l'intervalle de (23 ± 5) °C et à une humidité relative de (45 ± 10) %.
Toutefois, les essais individuels doivent être réalisés dans des conditions stables de température en raison de l'exigence d'exactitude élevée du mesurage de la profondeur. Cela signifie que:
- les éprouvettes doivent atteindre la température ambiante avant d'être soumises à l'essai;
ISO 14577-1:2026(fr) - la machine d'essai doit avoir atteint une température opérationnelle stable (il convient de consulter le manuel d’utilisation); - la température ambiante, la température de l’instrument et la température d’essai doivent se situer dans l’intervalle pour lequel l’étalonnage de la machine est valable, et - les autres influences extérieures provoquant des changements de température pendant un essai individuel ont été contrôlées.
...