kSIST FprEN 13674-1:2026
(Main)Railway applications - Rail - Part 1: Vignole railway rails 46 kg/m and above
- Abstract
This document specifies Vignole railway rails of 46 kg/m and greater linear mass, for conventional and high speed railway track usage.
Pearlitic steel grades are specified covering a hardness range of 200 HBW to 440 HBW and include non heat treated non alloy steels, non heat treated alloy steels, and heat treated non alloy steels and heat treated alloy steels.
There are 24 rail profiles specified in this document.
Two classes of rail straightness are specified, differing in requirements for straightness, surface flatness and crown profile. Two classes of profile tolerances are specified.
- Status
- Not Published
- Public Enquiry End Date
- 31-May-2023
- Technical Committee
- IŽNP - Reilway applications
- Current Stage
- 5020 - Formal vote (FV) (Adopted Project)
- Start Date
- 19-Nov-2026
- Due Date
- 07-Jan-2027
- Completion Date
- 20-Nov-2026
kSIST FprEN 13674-1:2026 is the Slovenian draft adoption of prEN 13674-1, a CEN draft European standard for Vignole railway rails. It specifies rails of 46 kg/m and above for conventional and high-speed railway track, including the rail profiles, steel grades, manufacture, identification, type tests and acceptance tests used by rail producers, purchasers and test laboratories.
What does kSIST FprEN 13674-1:2026 specify?
kSIST FprEN 13674-1:2026 specifies Vignole railway rails with a linear mass of 46 kg/m and greater for railway track use. The standard covers pearlitic steel grades across a hardness range of 200 HBW to 440 HBW, 24 rail profiles, two rail straightness classes and two profile tolerance classes.
The document is organized into clauses for purchaser information, steel grades, profile data, manufacture, qualifying tests and acceptance tests. It is followed by annexes that give the rail profiles, test methods, gauges, inclusion rating method, and the route for introducing a new rail steel grade.
| Annex | What it covers |
|---|---|
| Annex A | Rail profiles and their dimensions, properties and masses |
| Annex B | Plane strain fracture toughness test method for rails |
| Annex C | Rail foot surface longitudinal residual stress method |
| Annex D | Limiting sulfur prints for segregation assessment |
| Annex E | Profile and drilling gauges |
| Annex F | Microscopic examination for non-metallic inclusions |
| Annex G | Minimum requirements for introducing a new rail steel grade |
| Annex H | Significant technical changes compared with the previous edition |
| Annex ZA | Relationship with EU Directive (EU) 2016/797 and the TSI |
What are the key requirements of kSIST FprEN 13674-1:2026?
kSIST FprEN 13674-1:2026 combines product definition, production control, type approval testing and routine acceptance testing. In practice, it tells a rail manufacturer what must be ordered, how the rail must be made and marked, which tests prove the design, and which checks release each production lot.
Purchaser data and product definition
Clause 4 requires the purchaser to state the rail profile, steel grade, profile class X or Y, straightness class A or B, rail length, end drilling details, any special treatment for bolt holes, cold stamping on the cut face, and any paint code requirements. This matters because the supplier cannot complete manufacture or marking correctly unless these order details are fixed up front.
Clause 5 and Table 1 define the steel grades and their hardness ranges, including R200, R220, R260, R260Mn, R320Cr, R335V, R350HT, R350LHT, R370CrHT and R400HT. In practice, this is the grade selection that links chemistry, heat treatment and the branding code on the rail.
Manufacture and identification
Clause 7 requires product integrity under factory production control, with documented evidence of continuing compliance. The introduction says this approach is aligned with EN ISO 9001, which matters because the rail is safety-critical and the maker must control production consistently.
Clause 7 also requires suitable blooms, scale removal, a cross-sectional limit between bloom and rolled rail, and two-stage roller straightening about the XX and YY axes. That means the rail is not only checked at the end, but also constrained by the way it is rolled and straightened.
Clause 7.4 requires permanent identification by branding and hot stamping, with cold stamping only on the cut face unless the purchaser agrees otherwise. The identification system must allow the rail to be traced back to the heat, strand and bloom position, which is important for traceability when a quality issue is investigated.
Qualifying tests
Clause 8 sets the qualifying tests that demonstrate the rail grade and process are fit for service. These include fracture toughness, fatigue crack growth rate, fatigue test, residual stress in the rail foot, treated rail hardness uniformity, segregation checks and other acceptance-test results.
The qualifying tests are repeated at least every five years and after any significant production process change, and the manufacturer tests only the 60E1/60E2 profile or the heaviest section produced. In practice, this is the type-approval gate before a grade or process can be supplied confidently.
Annex B gives the fracture toughness method, Annex C the residual stress method and Annex D the sulfur-print limits. These annexes matter because they turn performance claims into testable procedures and acceptance limits.
Acceptance tests during production
Clause 9 covers routine laboratory, dimensional and inspection tests during production. It includes chemical composition, hydrogen, microstructure, decarburisation, oxide cleanness, sulphur prints, hardness, tensile testing, profile tolerances, straightness, cutting and drilling, gauges, and internal and surface quality inspection.
For heat-treated rails, Clause 9 also checks hardness distribution along the rail length, while for all grades the rail must pass ultrasonic internal quality inspection and surface defect limits. In practice, this is the routine release system for each heat, sequence or tonnage lot.
Geometry, straightness and defect limits
Clause 9.2 sets profile tolerances, straightness, surface flatness, twist and drilling tolerances. Clause 9.4 adds the requirements for ultrasonic inspection and surface quality, including limits for hot marks, grooves, cold marks and surface microstructural damage.
This matters because the rail must fit the track geometry and remain free from defects that could reduce performance in service. The document also requires automatic inspection methods for flatness and internal quality, with dispute checks using defined gauges and straight edges.
Introducing a new rail steel grade
Annex G gives the route for introducing a new rail steel grade into EN 13674-1. It requires mechanical and metallurgical data, welding qualification, track testing and documentation to CEN, so a new grade is supported by laboratory, production and in-track evidence before it can be added.
What terms does kSIST FprEN 13674-1:2026 define?
- bloom - A semi-finished product from continuous casting with a square, rectangular or circular section.
- heat - The liquid steel melt from a converter or electric arc furnace, together with the blooms cast from it within the defined mixing zone.
- sequence - A run of heats of the same steel grade cast through tundishes, possibly in parallel.
- heat treated rail - A rail that has been accelerated cooled from the austenitizing temperature during the metallurgical transformation period.
- rolling process - The process from blooms leaving the heating furnace to the finishing pass.
- isothermal treatment process - Holding blooms at elevated temperature to reduce hydrogen content, also called sub critical diffusion annealing.
- qualifying test - A special test and criterion used to confirm service performance of rails.
- acceptance test - A routine process and product control test, normally applied on a heat, sequence or tonnage basis.
Who uses kSIST FprEN 13674-1:2026?
kSIST FprEN 13674-1:2026 is used by rail mills, steel producers, quality managers, test laboratories and railway purchasers. It is also relevant to railway infrastructure managers and railway authorities that buy or approve rail for conventional and high-speed track.
Manufacturers use it to choose steel grades, set rolling and straightening conditions, mark rails and plan qualifying and acceptance tests. Buyers use it to state the required profile, straightness class, drilling and marking details at order stage. Laboratories use it for fracture toughness, fatigue, residual stress, hardness, tensile, ultrasonic and surface quality testing.
What changed in kSIST FprEN 13674-1:2026 from the previous edition?
kSIST FprEN 13674-1:2026 supersedes SIST EN 13674-1:2011+A1:2017. The document states these significant technical changes:
- the number of rail profiles is 24 instead of 23
- a new steel grade, R335V, is introduced
- the minimum stamping depth is reduced from 0.5 mm to 0.4 mm
- 60E2 may also be used for the qualifying tests
- the predictive equation is moved from the qualifying tests section to the acceptance tests section
- oxygen is removed as an element to be controlled and measured
- the Brinell hardness test conditions are changed
- a new normative annex is added for introducing a new rail steel grade
- rail transition references are removed
- the foot toe thickness requirement is revised
Which standards are used with kSIST FprEN 13674-1:2026?
| Reference | What it contributes |
|---|---|
| EN 10163-1:2004 | Surface condition requirements for hot-rolled steel products, used for surface defect terminology |
| CEN/TR 10261:2018 | Guidance on standards for determining chemical composition of iron and steel |
| EN ISO 6506-1:2014 | Brinell hardness test method |
| EN ISO 6892-1:2019 | Tensile test method at room temperature |
| EN ISO 14284:2022 | Sampling and sample preparation for chemical analysis |
| EN ISO 80000-1:2022 | Quantities, units and rounding rules |
| ISO 1099:2017 | Axial force-controlled fatigue testing |
| ISO 4968:2022 | Sulphur print method for macrographic examination |
| ISO 12108:2018 | Fatigue crack growth rate method |
| ASTM E399-22 | Plane-strain fracture toughness method used in Annex B |
The introduction also refers to EN ISO 9001 as the benchmark for factory quality assurance, and the bibliography names EN 10027-1 and EN 10027-2 for steel naming and numbering. Annex G also names EN 14587-1, EN 14587-2, EN 14730-1 and EN 15594 for welding and weld repair qualification.
What does the kSIST FprEN 13674-1:2026 document contain?
kSIST FprEN 13674-1:2026 contains a rail profile catalogue, steel grade tables, chemical and mechanical property tables, and dimensional tolerance tables. It also contains defined test methods and procedures for fracture toughness, fatigue crack growth, fatigue life, residual stress, sulphur prints, inclusions, hardness, tensile properties, ultrasonic inspection and surface quality.
The annexes add drawings of rail profiles, test-piece locations, calibration defects, gauges and evaluation diagrams. Several parts use figures and formulas to show where to cut test pieces, how to place strain gauges, how to calculate residual stress, and how to rate non-metallic inclusions.
Relations
- Effective Date
- 18-Jan-2023
Get Certified
Connect with accredited certification bodies for this standard

IRIS Certification (UNIFE)
International Railway Industry Standard certification.

TÜV SÜD Rail GmbH
TÜV SÜD railway certification services.

Bureau Veritas Railway Certification
Railway and transportation certification.
Sponsored listings
Frequently Asked Questions
kSIST FprEN 13674-1:2026 is a draft published by the Slovenian Institute for Standardization (SIST). Its full title is "Railway applications - Rail - Part 1: Vignole railway rails 46 kg/m and above". This standard covers: This document specifies Vignole railway rails of 46 kg/m and greater linear mass, for conventional and high speed railway track usage. Pearlitic steel grades are specified covering a hardness range of 200 HBW to 440 HBW and include non heat treated non alloy steels, non heat treated alloy steels, and heat treated non alloy steels and heat treated alloy steels. There are 24 rail profiles specified in this document. Two classes of rail straightness are specified, differing in requirements for straightness, surface flatness and crown profile. Two classes of profile tolerances are specified.
This document specifies Vignole railway rails of 46 kg/m and greater linear mass, for conventional and high speed railway track usage. Pearlitic steel grades are specified covering a hardness range of 200 HBW to 440 HBW and include non heat treated non alloy steels, non heat treated alloy steels, and heat treated non alloy steels and heat treated alloy steels. There are 24 rail profiles specified in this document. Two classes of rail straightness are specified, differing in requirements for straightness, surface flatness and crown profile. Two classes of profile tolerances are specified.
kSIST FprEN 13674-1:2026 is classified under the following ICS (International Classification for Standards) categories: 45.080 - Rails and railway components; 93.100 - Construction of railways. The ICS classification helps identify the subject area and facilitates finding related standards.
kSIST FprEN 13674-1:2026 has the following relationships with other standards: It is inter standard links to SIST EN 13674-1:2011+A1:2017. Understanding these relationships helps ensure you are using the most current and applicable version of the standard.
kSIST FprEN 13674-1:2026 is associated with the following European legislation: EU Directives/Regulations: 2016/797/EU; Standardization Mandates: M/483, M/591. When a standard is cited in the Official Journal of the European Union, products manufactured in conformity with it benefit from a presumption of conformity with the essential requirements of the corresponding EU directive or regulation.
kSIST FprEN 13674-1:2026 is available in PDF format for immediate download after purchase. The document can be added to your cart and obtained through the secure checkout process. Digital delivery ensures instant access to the complete standard document.
Standards Content (Sample)
Contents
- Introduction
- 1 Scope
- 2 Normative references
- 3 Terms and definitions
- 3.1 bloom
- 3.2 heat
- 3.3 sequence
- 3.4 heat treated rail
- 3.5 rolling process
- 3.6 isothermal treatment process
- 3.7 qualifying test
- 3.8 acceptance test
- 3.9 rail running surface
- 3.10 units of measurement
- 4 Information to be supplied by the purchaser
- 5 Steel grades
- 6 Profile drawings/properties/mass
- 7 Manufacture
- 7.1 Product integrity
- 7.2 Blooms
- 7.3 Rails
- 7.4 Identification
- 8 Qualifying tests
- 8.1 Procedure
- 8.2 Fracture toughness (K )
- 8.3 Fatigue crack growth rate
- 8.4 Fatigue test
- 8.5 Residual stress in rail foot
- 8.6 Treated rails
- 8.7 Segregation
- 8.8 Other qualifying requirements
- 9 Acceptance tests
- 9.1 Laboratory tests
- 9.2 Dimension tolerances
- 1 V and H: Location of flatness measurements 1 overlap
- 9.3 Gauges
- 9.4 Inspection for internal quality and surface quality
- 1 Drilling Diameter
- 2 Squareness of ends 0,6 mm in any direction
- 3 Length
- Annex A
- Annex B
- Annex C
- Annex D
- Annex E
- 1 HF = fishing height (see Figure E.1) and
- Annex F
- Annex G
- Annex H
- 1. The number (nine) of pearlitic steel grades is suppressed
- 3.3 The condition "if the caster has many strands" to authorise to use different tundish
- 3.4 Suppress the former item 3.4 "re-heated rail"
- 5 The sentence "For inclusion of a new rail steel grade in this standard, the supplier
- 26 MPam for minimum individual values
- 29 MPam for the minimum mean value
- 8.7 New numbering (was 8.8)
- 8.8 New numbering (was 8.9)
- Annex G New normative annex “Minimum requirements for the introduction of a new rail
- Annex H Updated
- Annex ZA Text modified
- Annex ZA
- Bibliography
Introduction
This Introduction provides an explanation of the concepts and reasoning considered for this standard. Whenever possible this part of EN 13674 is performance based, recognizes the European Quality System standard EN ISO 9001 and requires manufacturers to offer the latest proven technology to consistently satisfy the demanding quality of the required product.
This part of EN 13674 has two major divisions:
1) qualifying tests; 2) acceptance tests.
The qualifying tests take into account performance requirements. They also include typical results from relevant acceptance tests.
The acceptance tests control those characteristics of the rail steel and rail that are of relevance to the production of high quality rails including heat treated rails and the demands of the railway. To ensure the supply of high quality rails, some restrictions on production processes are considered. The performance based standard applies to all procurements falling inside the requirements of the European th Procurement Directive (93/38/EEC of 14 June 1993), taking into account safety implications and at the same time addressing modern production technology and the requirements of high-speed railways. As a result of the Directive it was recognized that there would be few opportunities (and these would have to be for transparent safety considerations) for derogation from the standard to operate between the user and the manufacturer.
The standard includes a prerequisite for all manufacturers to prove conformity against a set of qualifying test criteria. Qualifying tests include all "normal" acceptance test results plus new "type-casting" features such as fracture toughness, fatigue cracks growth rate, fatigue test and residual stress. To provide users with the necessary confidence, acceptance limits have been based on results from rail known to have performed well in demanding track installations.
The standard includes a quality assurance and inspection clause as part of product integrity. In order that quality management systems are consistent across all manufacturers and that users have the best assurance for the consistency of required product quality on this safety critical component of the track, this rail standard recommends that the manufacturers' quality assurance systems are at least equivalent to the requirements of EN ISO 9001. The inclusion of this requirement also reduces the need to incorporate detailed method and calibration descriptions on items such as normal chemical composition determination and the need to define more extensive testing.
oSIST prEN 13674-1:2023 prEN 13674-1:2023 (E)
1 Scope
This document specifies Vignole railway rails of 46 kg/m and greater linear mass, for conventional and high speed railway track usage.
Pearlitic steel grades are specified covering a hardness range of 200 HBW to 440 HBW and include non heat treated non alloy steels, non heat treated alloy steels, and heat treated non alloy steels and heat treated alloy steels.
There are 24 rail profiles specified in this document.
Two classes of rail straightness are specified, differing in requirements for straightness, surface flatness and crown profile. Two classes of profile tolerances are specified.
2 Normative references
The following documents are referred to in the text in such a way that some or all of their content constitutes requirements of this document. For dated references, only the edition cited applies. For undated references, the latest edition of the referenced document (including any amendments) applies. EN 10163-1:2004, Delivery requirements for surface condition of hot-rolled steel plates, wide flats and sections - Part 1: General requirements CEN/TR 10261:2018, Iron and steel - European standards for the determination of chemical composition EN ISO 6506-1:2014, Metallic materials - Brinell hardness test - Part 1: Test method (ISO 6506-1:2014) EN ISO 6892-1:2019, Metallic materials - Tensile testing - Part 1: Method of test at room temperature (ISO 6892- 1:2019) EN ISO 14284:2022, Steel and iron - Sampling and preparation of samples for the determination of chemical composition (ISO 14284:2022) EN ISO 80000-1:2022, Quantities and units - Part 1: General (ISO 80000-1:2022) ISO 1099:2017, Metallic materials - Fatigue testing - Axial force-controlled method ISO 4968:2022, Steel - Macrographic examination by sulphur print (Baumann method) ISO 12108:2018, Metallic materials - Fatigue testing - Fatigue crack growth method ASTM E399-22, Standard test method for linear-elastic plane-strain fracture toughness of metallic materials
3 Terms and definitions
For the purposes of this document, the following terms and definitions apply. ISO and IEC maintain terminology databases for use in standardization at the following addresses:
- IEC Electropedia: available at https://www.electropedia.org/
- ISO Online browsing platform: available at https://www.iso.org/obp
3.1 bloom
refers to a semi product produced from a continuous casting machine with either a square, rectangular or circular section
oSIST prEN 13674-1:2023 prEN 13674-1:2023 (E)
3.2 heat
liquid steel melt tapped out of a converter or electric arc furnace which includes after continuous casting a given number of blooms relating to the weight of the heat and the extension of the mixing zone Note 1 to entry: In the case of sequence casting the blooms belonging to the mixing zone should be clearly defined.
3.3 sequence
any number of heats, of the same steel grade, which undergo continuous casting in tundishes Note 1 to entry: Tundishes may be used in parallel.
3.4 heat treated rail
rail that has undergone accelerated cooling from austenitizing temperature during the metallurgical transformation period Note 1 to entry: The heat treatment can be carried out directly after rolling or following a separate reheating process to achieve the austenitization temperature.
3.5 rolling process
process between the blooms leaving the heating furnace and exiting the finishing pass
3.6 isothermal treatment process
process whereby blooms are held for a period of time at an elevated temperature for reducing the hydrogen content Note 1 to entry: For maximum efficiency this is as near to (but below) the austenite to pearlite transformation temperature as is practically possible.
Note 2 to entry: This process is sometimes referred to as sub critical diffusion annealing.
3.7 qualifying test
special test and criteria which are relevant to some aspects of the service performance of rails Note 1 to entry: Acceptance tests also form part of the qualifying tests.
3.8 acceptance test
test carried out as part of the process and product control system, normally on a heat, sequence or tonnage basis
3.9 rail running surface
curved surface of the rail head. Area between both gauge corners (transition points of the head inclination and the first head radius)
3.10 units of measurement
for the purpose of determining conformance with the specification, numeric values are rounded according to the rules stipulated in EN ISO 80000-1:2022
oSIST prEN 13674-1:2023 prEN 13674-1:2023 (E)
4 Information to be supplied by the purchaser
The purchaser shall provide the supplier with the following information at the time of tender or order:
a) rail profile (see Annex A); b) steel grade (see Clause 5); c) profiles class, ‘X’ or ‘Y’ (see 9.2.1); d) straightness class ‘A’ or ‘B’ of rail as specified in 9.2.2; e) length(s) of rail (see Table 9); f) undrilled or drilled rail ends to take fish bolts, and location and dimensions of holes when required (see 9.2.3); g) any special treatment to be applied to bolt holes and corresponding special tolerances for bolt holes (see 9.2.3); h) cold stamping on the cut face (see 7.4.3); i) paint code requirements (see 7.4.4).
5 Steel grades
The applicable steel grades are given in Table 1. The hardness ranges of the steel grades shall conform to those given in Table 1.
For the steel grades in Table 1, the steel names and steel numbers were allocated in accordance with EN 10027-1 and EN 10027-2, respectively.
For inclusion of a new rail steel grade in this document, the supplier shall comply with the requirements of Annex G “Minimum requirements for the introduction of a new rail steel grade in EN 13674-1”.
oSIST prEN 13674-1:2023 prEN 13674-1:2023 (E) Table 1 — Steel grades a Steel grade Hardness range Description Branding lines (HBW) Steel name Steel number Non-alloy No branding lines R200 1.0521 200 to 240 Non heat treated
Non-alloy R220 1.0524 220 to 260 Non heat treated ————
Non-alloy —— R260 1.0623 260 to 300 Non heat treated ————
Non-alloy Mn ———— R260Mn 1.0624 260 to 300 Non heat treated ————
Alloy (Cr, Si) ———— R320Cr 1.0915 320 to 360 Non heat treated ————
Alloy (V, Si) __________ Non heat treated __________ R335V 1.0639 335 - 375
Non-alloy —— b R350HT 1.0631 350 to 390 Heat treated ———— ————
Non-alloy —— b R350LHT 1.0632 350 to 390 Heat treated ———— ————
Alloy Cr)) —— R370CrHT 1.0992 370 to 410 Heat treated ———— ————
Non-alloy ———— R400HT 1.1254 400 to 440 Heat treated ———— ————
a See Table 5 a) and Table 5 b) for chemical composition/mechanical properties. b See Table 6 for hardness requirements.
6 Profile drawings/properties/mass
Rail profiles, dimensions, properties and linear masses shall be in accordance with Annex A. The tolerances of certain dimensions shall be as given in Table 7. All other quantities are informative only.
NOTE Linear masses have been calculated based on the density of steel of 7,85 kg/dm .
oSIST prEN 13674-1:2023 prEN 13674-1:2023 (E)
7 Manufacture
7.1 Product integrity
Rails shall be produced under a comprehensive system of factory production control which shall ensure confidence in the conformity of the finished product. The system shall address this document to ensure that the finished products consistently comply with requirements to achieve the product integrity necessary to provide assurance of product safety in track.
Manufacturers shall demonstrate continuing compliance, including documented evidence, with the factory production control system required.
NOTE Manufacturers having a factory production control system which complies with EN ISO 9001 are recognized as satisfying the minimum requirements specified by this clause.
7.2 Blooms
Blooms made from basic oxygen steel or electric arc furnace steel that has been secondary ladle arc refined, vacuum degassed and continuously cast, shall be used for the manufacture of rails.
7.3 Rails
7.3.1 The manufacturer shall operate a procedure for the effective removal of scale during the
manufacturing process.
7.3.2 The cross-sectional area of the rail shall not exceed one ninth that of the bloom from which the rail is rolled.
7.3.3 Rail straightening shall be by a two stage roller straightening process which straightens the rail about its XX and YY axes as defined in the rail profiles shown in Annex A. End deviations or a localised deviation on the rail may be corrected using pressing.
NOTE Other mandatory processes are described in the relevant clauses within the document.
7.4 Identification
7.4.1 Branding
Brand marks shall be rolled in relief on one side and in the middle of the web (see Annex A) of each rail at least once every 4 m. The brand marks on the rails shall be clearly legible and shall be 20 mm to 25 mm high, raised between 0,6 mm and 1,3 mm.
The branding line(s) to denote grade shall be 50 mm in length for the long branding line and 25 mm in length for the short branding line.
The brand marks shall include:
a) identification of the mill; b) steel grade as shown in Table 1; c) last two figures of the year of manufacture; d) rail profile identification as shown in Annex A.
oSIST prEN 13674-1:2023 prEN 13674-1:2023 (E) EXAMPLES
ROLLING MILL _______ 07 60 E1
(60 E1 profile rail rolled 2007, non-alloy rail steel grade R260).
ROLLING MILL _______ _______ 07 60 E1
(60 E1 profile rail rolled 2007, non-alloy heat treated rail steel grade R350HT). NOTE The sequence of the branding marks is at the discretion of the manufacturer.
7.4.2 Hot stamping
In addition to the branding requirements of 7.4.1, each rail shall be identified by a numerical and/or alphabetical code system, hot stamped on the non-branded side of the rail web by machine and each rail shall be hot stamped at least once every 10 m.
The figures and letters used shall be clearly legible and shall be 16 mm high. The stamped characters shall have a flat or radius face (1 mm to 1,5 mm wide) with bevels on each side. The letters and numbers shall be on a 10° angle from vertical and shall have rounded corners. The stamping shall be between 0,4 mm and 1,5 mm in depth along the middle of the web as defined for the branding in annex A. The design shall be as shown in Figure 1.
Figure 1 — Design of letters and numbers on a 10° angle for rail stamps The identification system employed shall be such as to enable the hot stamped marking to be collated with the:
a) number of the heat from which the rail has been rolled; b) number of the strand and position of bloom within the strand; c) position of the rail in the bloom (A, B ... Y).
In the event of identification marks having been removed, omitted or requiring alteration, re-identification of such marks shall be made by rotary burr or other method agreed by the customer. NOTE 1 A rail can display different indications of position of the rail in the bloom (A,B…Y) along its length. NOTE 2 Subsequent cutting could result in more than one rail length having the same identity.
oSIST prEN 13674-1:2023 prEN 13674-1:2023 (E)
7.4.3 Cold stamping
Cold stamping may only be used on the cut face of the rail within the central portion of the head. Cold stamping at another position shall be agreed by the purchaser.
7.4.4 Other identification
The purchaser shall specify their requirements for any colour coding or special marking instructions and their position on the rail at the time of enquiry or order.
8 Qualifying tests
8.1 Procedure
8.1.1 The manufacturer shall describe any bloom slow cooling or isothermal treatment process used to demonstrate compliance with the requirements of 9.1.3.2.
8.1.2 All qualifying tests as specified in 8.2 to 8.8 shall be undertaken at least once every five years and as a result of any significant production process change for all grades. The manufacturer shall only carry out testing on the 60E1/60E2 profile or the heaviest section produced. All rail grades and profiles supplied shall conform to the qualifying criteria in accordance with 8.2 to 8.8. The results for the grades to be supplied shall be provided at the time of tendering. In the event of a manufacturer not having produced the rail grade prior to the tender enquiry he shall have the option of carrying out such tests on the first available sequence. When the qualifying criteria have been complied with, compliance with the standard is demonstrated and consequently the manufacturer is qualified. 8.1.3 The samples in accordance with 8.1.4 and 8.1.5 shall be removed from finished roller straightened rails. These samples shall not be subject to any further mechanical or thermal treatment (other than the treatment of ageing of the tensile test pieces as described in 9.1.9.2). 8.1.4 Test pieces for fracture toughness, fatigue crack growth rate and fatigue tests (see 8.2, 8.3 and 8.4 respectively) shall be taken from at least 3 sample rails taken at a minimum of 3 m from the cut ends of the rail. Sample rails shall be from different heats.
8.1.5 For residual stress tests (see 8.5), there shall be 6 sample rails and the test pieces shall be taken at least 3 m from each rail end. Sample rails shall be from at least 3 different heats. 8.1.6 All tests should be carried out by a laboratory that operates an approved and audited quality assurance system conforming to requirements at least equivalent to EN ISO 9001. 8.1.7 The purchaser shall have access to all test records, calibrations and calculations that contribute to the final results.
8.1.8 All test results shall be reported to the purchaser.
8.2 Fracture toughness (K )
Ic
8.2.1 Test pieces and test methods
Tests shall be performed in accordance with Annex B.
8.2.2 Qualifying criteria
The value of K shall comply with Table 2.
Ic
oSIST prEN 13674-1:2023 prEN 13674-1:2023 (E) Table 2 — Minimum single and minimum mean values of K Ic Minimum single value Minimum mean value Steel grade 1/2 1/2 K (MPa m ) K (MPa m ) Ic Ic R200 and R220 30 35 R260 and R260Mn 26 29 R320Cr 24 26 R335V 26 29 R350HT 30 32 R350LHT, R370CrHT, R400HT 26 29
NOTE In some circumstances K values can be used for the purpose of qualification, see B.6. Q
8.3 Fatigue crack growth rate
8.3.1 Test method
Tests shall be carried out in accordance with the general requirements of ISO 12108:2018.
8.3.2 Test pieces
A three points bend, single edge notch test piece, of the dimensions and location within the rail shown in Figure 2 shall be used.
8.3.3 Number of tests and test conditions
A minimum of 3 tests from each sample rail shall be performed under the following conditions:
- test temperature shall be within the range +15 °C to +25 °C;
- R = 0,5 (R = minimum cyclic load/maximum cyclic load);
- 3 points bend test piece loading span shall be 4 W (see Figure 2);
- cyclic loading frequency shall be within the range 15 Hz to 40 Hz;
- environment: laboratory air.
8.3.4 Qualifying criteria
Fatigue crack growth rates (m/Gc) shall not exceed the values given in Table 3. Table 3 — Fatigue crack growth rates
Steel grades Δ K = 10 MPa m Δ K = 13,5 MPa m All grades 17 m/Gc 55 m/Gc
oSIST prEN 13674-1:2023 prEN 13674-1:2023 (E)
8.4 Fatigue test
8.4.1 Test method
Constant amplitude fatigue tests shall be carried out in accordance with ISO 1099:2017 or ISO 12106. In case of testing carried out according to ISO 1099:2017, a minimum of 50 initial fatigue cycles under strain control shall be applied to define the load necessary to achieve the required strain.
8.4.2 Test pieces
The test pieces shall be machined from the sample rail as shown in Figure 3.
8.4.3 Number of tests and test conditions
A minimum of 3 test pieces shall be tested from each sample rail under the following conditions:
- test temperature shall be within the range + 15 °C to + 25 °C;
- control variable shall be axial strain amplitude of load;
- strain or load cycle shall be symmetrical about the initial, zero load. R ratio to be used is -1.
8.4.4 Qualifying criteria
For an amplitude of total strain of 0,00135, the life of each specimen shall be greater than 5 × 10 cycles. NOTE Life is defined as the number of cycles up to the complete separation of the specimen.
8.5 Residual stress in rail foot
8.5.1 Test method
The residual stresses in the rail foot shall be determined in accordance with Annex C.
8.5.2 Test pieces
Each of the 6 test pieces from the rail section shall be 1,00 -0/+0,10 m in length and shall be taken from rails as described in 8.1.3 and 8.1.5.
NOTE Only a small part of the test piece will be destroyed for the purpose of measuring residual stress; the remainder can be used for other qualifying approval tests.
8.5.3 Measurements
Longitudinal residual stress determinations shall be made on the rail foot of each of the 6 test pieces described in 8.5.2. The location of the measurements is shown in Figure C.1. If data are available for straightness class A rails then class B rails of the same profile need not be tested.
8.5.4 Qualifying criteria
The maximum longitudinal residual stress in the foot shall be +250 MPa (tensile stresses) for all steel grades.
oSIST prEN 13674-1:2023 prEN 13674-1:2023 (E)
...