ISO/DTS 23879
(Main)Nanotechnologies — Structural characterization of graphene oxide flakes — Thickness and lateral size measurement using atomic force microscopy and scanning electron microscopy
- Abstract
This document describes methods for measuring the lateral size and thickness of graphene oxide (GO) flakes using scanning electron microscopy (SEM) and atomic force microscopy (AFM) respectively, including sample pre-treatments, measurement procedures and data analysis. It is applicable to the characterization of graphene oxide in powder and liquid dispersion forms.
- Status
- Not Published
- Technical Committee
- ISO/TC 229 - Nanotechnologies
- Current Stage
- 5020 - Proof sent to secretariat or FDIS ballot initiated: 8 weeks - 50 Approval
- Start Date
- 27-Oct-2026
- Due Date
- 27-Oct-2026
- Completion Date
- 27-Oct-2026
Buy Documents
ISO/DTS 23879 - Nanotechnologies — Structural characterization of graphene oxide flakes — Thickness and lateral size measurement using atomic force microscopy and scanning electron microscopy
REDLINE ISO/DTS 23879 - Nanotechnologies — Structural characterization of graphene oxide flakes — Thickness and lateral size measurement using atomic force microscopy and scanning electron microscopy
ISO/DTS 23879 is an ISO draft technical specification for structural characterization of graphene oxide (GO) flakes. It specifies how to measure GO flake lateral size with scanning electron microscopy (SEM) and thickness with atomic force microscopy (AFM), including sample preparation, image acquisition, data analysis, and reporting for powder and liquid dispersion forms.
What does ISO/DTS 23879 specify?
ISO/DTS 23879 specifies a measurement workflow for GO flakes in powder and liquid dispersion forms. The document focuses on dimensional characterization, with SEM used for lateral size and AFM used for thickness, and it also gives the sample-preparation and analysis steps needed to make results comparable.
The document is organized into nine clauses and four informative annexes:
| Annex | What it covers |
|---|---|
| Annex A | Characterization descriptors for lateral size and shape of GO flakes using SEM |
| Annex B | VAMAS interlaboratory comparison study on GO lateral size using SEM |
| Annex C | Results of an AFM VAMAS interlaboratory comparison study |
| Annex D | Example of a test report |
Clause 5 gives the overall measurement sequence. It points users to SEM first for lateral size, then AFM for thickness, and notes that if confirmation of GO presence is needed, ISO/TS 21356-1 and ISO/TS 23356 are used.
What are the key requirements of ISO/DTS 23879?
ISO/DTS 23879 sets out practical requirements that affect how samples are prepared, how instruments are run, and how results are analysed. The main point is to reduce bias from sample handling and flake selection so that the reported size and thickness values are representative.
Sample preparation matters before either method
Clause 6 requires GO to be deposited on a clean substrate with good separation between flakes. Powder samples are first dispersed in a suitable solvent, and the document recommends low-shear mixing; ultrasonication should be avoided where possible because it can break sheets and shift the measured size distribution.
For GO dispersions, the document recommends a concentration of 0.05 mg/mL before further dilution. For SEM, samples are prepared on a clean silicon wafer with a minimal oxide layer, while AFM samples are prepared on freshly cleaved mica. Drying is done at room temperature for at least 20 minutes in a clean environment.
SEM is used to measure lateral size
Clause 7 says SEM should be done with a field-emission instrument that is dimensionally calibrated with traceable standards. A secondary electron detector with better than 10 nm resolution is recommended, and the accelerating voltage should be 3 kV or less, using the lowest voltage that still gives clear flake boundaries.
The method also requires a representative set of flakes across the substrate. More than 200 randomly chosen flakes should be imaged and suitable for analysis. This matters because the document says flake selection is usually the biggest source of bias, more than the instrument limits themselves.
Only suitable flakes are measured
Clause 7 identifies flakes that can and cannot be used. Suitable flakes are isolated flakes, flakes whose edges just touch but remain distinguishable, and overlapping flakes whose borders can still be separated. Unsuitable cases include dense clusters, bulky graphitic particles, and folded flakes with substantial folded areas.
In practice, this means the analyst has to inspect image quality and edge clarity before measuring. The standard is aimed at representative dimensional data, not at forcing every visible object into the result set.
SEM data can be analysed in two ways
Clause 7.3 allows two analysis approaches. The first is perimeter tracing, either manual or automated, from which area, perimeter, Feret diameters, ellipse axes, and equivalent circular diameter (ECD) can be obtained. The second is direct measurement of length and width using the perpendicular bisector approach.
The document recommends reporting the analysis type used, because different descriptors describe shape in different ways. Annex A supports this by identifying ECD, LR, and Cl as useful size and shape descriptors for GO flakes.
AFM is used for thickness, with a defined calibration and scan setup
Clause 8 requires AFM scanners to be z-calibrated with traceable step-height standards in accordance with ISO 11952. The z-axis resolution should be 0.1 nm or better, and the instrument should be used in closed-loop intermittent contact mode in ambient conditions.
The document also gives practical scan guidance: a test scan of 10 µm × 10 µm, a scan rate of 0.8 Hz or lower, and 256 × 256 pixels, followed by larger-area scanning to locate flakes and smaller scans to image individual flakes. At least 10 flakes should be obtained for a representative set.
AFM thickness is calculated from height distributions
Clause 8.3 recommends the histogram method for GO flakes. The topography is flattened by removing tilt, bow, and scan-line artefacts, then a height profile is turned into a height probability distribution histogram. Two Gaussian peaks are fitted, one for substrate and one for flake, and the thickness is the difference between their maximum frequency height values.
This matters because GO flakes are thin and their measured height can be influenced by noise, contamination, and background shape. The document therefore calls for at least three height profiles per flake and statistics across at least 10 flakes.
Reporting is part of the method
Clause 9 requires the report to include the test date, environmental conditions, sample description, the standard and method used, instrument and imaging descriptors, measurement descriptors, averages and ranges, thickness with associated uncertainty, any deviations, and unusual features. Annex D gives an example test report format.
What terms does ISO/DTS 23879 define?
ISO/DTS 23879 uses a small set of defined terms and abbreviations that are central to the method.
- AFM - atomic force microscopy, a surface-imaging method that uses a sharp tip on a cantilever to build a height image.
- SEM - scanning electron microscopy, a method that scans the surface with an electron beam and analyses the emitted signals to image structure and topography.
- GO - graphene oxide, chemically modified graphene prepared by oxidation and exfoliation of graphite.
- ECD - equivalent circular diameter, the diameter of a circle with the same area as the flake.
- LR - the ratio of major axis to minor axis lengths of the equivalent ellipse, used as a shape descriptor.
- Cl - compactness relative to the major axis length of the equivalent ellipse, used to describe flake shape.
- H - the difference in maximum frequency height values of sample and substrate, used as the AFM thickness result.
Who uses ISO/DTS 23879?
ISO/DTS 23879 is aimed at the GO supply chain and at laboratories that need repeatable GO flake measurements. It is useful for technical teams working on powders and dispersions, including suppliers, buyers, quality managers, and R&D staff who need comparable size and thickness data.
The document is also relevant in application areas where GO flake dimensions affect performance, such as composites, catalysts, supercapacitors, Li-ion batteries, nanofluids, and corrosion-protection-related materials. In practice, users apply it for material characterization, incoming inspection, method validation, and interlaboratory comparison work.
Which standards are used with ISO/DTS 23879?
ISO/DTS 23879 relies on a small set of standards and related documents that support terminology, calibration, and broader particle characterization.
- ISO 18115-2 - provides scanning-probe microscopy vocabulary used in the terms and definitions.
- ISO/TS 80004-13 - provides graphene and related 2D materials vocabulary used for GO terminology.
- ISO/TS 21356-1 - is referenced when confirmation of GO presence is required for powders and dispersions.
- ISO/TS 23356 - is also referenced for confirming the presence of GO.
- ISO 11952 - provides the calibration basis for AFM geometric measurements and step-height standards.
- ISO 19749 - gives general guidance for particle size and shape distributions measured by SEM.
What does the ISO/DTS 23879 document contain?
ISO/DTS 23879 contains a worked measurement procedure rather than only a short requirement list. It includes an overview figure showing the sequence of SEM and AFM measurements, detailed sample-preparation steps, recommended imaging settings, and the two SEM analysis approaches with their output descriptors.
The AFM part includes scan setup guidance, the histogram-based height analysis method, and the calculation route for flake thickness. The annexes add useful context: Annex A discusses descriptors, Annex B and Annex C summarize interlaboratory comparison work, and Annex D provides a test report example with record sheets for SEM and AFM data.
Buy Documents
ISO/DTS 23879 - Nanotechnologies — Structural characterization of graphene oxide flakes — Thickness and lateral size measurement using atomic force microscopy and scanning electron microscopy
REDLINE ISO/DTS 23879 - Nanotechnologies — Structural characterization of graphene oxide flakes — Thickness and lateral size measurement using atomic force microscopy and scanning electron microscopy
Frequently Asked Questions
ISO/DTS 23879 is a draft published by the International Organization for Standardization (ISO). Its full title is "Nanotechnologies — Structural characterization of graphene oxide flakes — Thickness and lateral size measurement using atomic force microscopy and scanning electron microscopy". This standard covers: This document describes methods for measuring the lateral size and thickness of graphene oxide (GO) flakes using scanning electron microscopy (SEM) and atomic force microscopy (AFM) respectively, including sample pre-treatments, measurement procedures and data analysis. It is applicable to the characterization of graphene oxide in powder and liquid dispersion forms.
This document describes methods for measuring the lateral size and thickness of graphene oxide (GO) flakes using scanning electron microscopy (SEM) and atomic force microscopy (AFM) respectively, including sample pre-treatments, measurement procedures and data analysis. It is applicable to the characterization of graphene oxide in powder and liquid dispersion forms.
ISO/DTS 23879 is classified under the following ICS (International Classification for Standards) categories: 07.120 - Nanotechnologies. The ICS classification helps identify the subject area and facilitates finding related standards.
ISO/DTS 23879 is available in PDF format for immediate download after purchase. The document can be added to your cart and obtained through the secure checkout process. Digital delivery ensures instant access to the complete standard document.
Standards Content (Sample)
Contents
- Introduction
- 1 Scope
- 2 Normative references
- 3 Terms and definitions
- 3.1 atomic force microscopy
- 3.2 scanning electron microscopy
- 3.3 graphene oxide
- 4 Abbreviated terms
- 5 Overview
- 6 Sample preparation
- 7 Scanning electron microscopy
- 7.1 General
- 7.2 Imaging
- 7.3 Data analysis
- 8 Atomic force microscopy
- 8.1 General
- 8.2 Method
- 8.3 Image and data analysis to obtain flake height
- 9 Reporting
- Annex A
- Annex B
- Annex C
- Annex D
- 1 Name of Operator
- 2 Sample Description
- 3 Instrument name/details
- 4. Instrument calibration details (sample, date, etc)
- 5. Instrument imaging descriptors
- 6. Data analysis
- 7. Data recording (see Table D.1 and Table D.2)
- Bibliography
Introduction
Graphene oxide (GO) is an oxidized form of graphene functionalised with oxygen-containing groups. It is a single layer two-dimensional material with an oxygen-to-carbon ratio of approximately 0,5, which is prepared by oxidation and exfoliation of graphite, causing extensive oxidative modification of the basal plane. The benefits of this material have been shown for many fields such as catalysts, supercapacitors, Li- [1]-[4] ion batteries, nanofluids and composites. GO flakes come in many different sizes and shapes, thus when [5],[6] GO is incorporated into a macroscopic material, these differences affect the material’s properties. For example, lateral flake size has a significant influence on mechanical properties and corrosion protection [7]-[10] when GO is used in composite materials.
Scanning electron microscopy (SEM) is a key technique for the visualization of GO flakes and measurement of their lateral sizes. The sample pre-treatment, the collection of micrographs and the procedures for the image analysis require a standardized method to ensure the consistency and reliability of reported material properties.
Atomic force microscopy (AFM) is a powerful technique for the measurement of features at the nanoscale. For GO, this includes flake thickness and lateral size. However, although the theoretical value of single-layer GO is known, in reality measurement uncertainties due to contaminants and instrument noise can be large, such that the thickness can not be accurately measured by common data processing methods. Therefore, it is highly desirable to standardize a method to ensure the consistency and reliability of measurement results. This document describes the methodology for measuring the lateral size and thickness of GO flakes using SEM and AFM, respectively. It aims to provide a reliable measurement methodology for determining GO lateral size and thickness, that can be used by the GO supply chain.
FINAL DRAFT Technical Specification ISO/DTS 23879:2026(en) Nanotechnologies — Structural characterization of graphene oxide flakes — Thickness and lateral size measurement using atomic force microscopy and scanning electron microscopy
1 Scope
This document describes methods for measuring the lateral size and thickness of graphene oxide (GO) flakes using scanning electron microscopy (SEM) and atomic force microscopy (AFM), respectively, including sample pre-treatments, collection of micrographs and data analysis. It is applicable to the characterization of GO in powder and liquid dispersion forms.
2 Normative references
The following documents are referred to in the text in such a way that some or all of their content constitute requirements of this document. For dated references, only the edition cited applies. For undated references, the latest edition of the referenced document (including any amendments) applies. ISO 18115-2, Surface chemical analysis — Vocabulary — Part 2: Terms used in scanning-probe microscopy ISO/TS 80004-13, Nanotechnologies — Vocabulary — Part 13: Graphene and other two-dimensional (2D) materials
3 Terms and definitions
For the purposes of this document, the terms and definitions given in ISO 18115-2 and ISO/TS 80004-13 and the following apply.
ISO and IEC maintain terminology databases for use in standardization at the following addresses:
- ISO Online browsing platform: available at https:// www .iso .org/ obp
- IEC Electropedia: available at https:// www .electropedia .org/
3.1 atomic force microscopy
AFM method for imaging surfaces by mechanically scanning their surface contours, in which the deflection of a sharp tip sensing the surface forces, mounted on a compliant cantilever, is monitored Note 1 to entry: AFM can provide a quantitative height image of both insulating and conducting surfaces. Note 2 to entry: Some AFM instruments move the sample in the x-, y- and z-directions while keeping the tip position constant and others move the tip while keeping the sample position constant. Note 3 to entry: AFM can be conducted in vacuum, a liquid, a controlled atmosphere or air. Atomic resolution may be attainable with suitable samples, with sharp tips and by using an appropriate imaging mode. Note 4 to entry: Many types of force can be measured, such as the normal forces or the lateral, friction or shear force. When the latter is measured, the technique is referred to as lateral, frictional or shear force microscopy. This generic term encompasses all of these types of force microscopy.
Note 5 to entry: AFMs can be used to measure surface-normal forces at individual points in the pixel array used for imaging.
ISO/DTS 23879:2026(en) Note 6 to entry: For typical AFM tips with radii <100 nm, the normal force should be less than about 0,1 μN, depending on the sample material, or irreversible surface deformation, and excessive tip wear occurs. [SOURCE: ISO 18115-2:2013, 3.2]
3.2 scanning electron microscopy
SEM method that examines and analyses the physical information (such as secondary electrons, backscattered electrons, absorbed electrons and x-ray radiation) obtained by generating electron beams and scanning the surface of the sample in order to determine the structure, composition and topography of the sample [SOURCE: ISO 80004-6:2021, 4.5.5]
3.3 graphene oxide
GO chemically modified graphene prepared by oxidation and exfoliation of graphite, causing extensive oxidative modification of the basal plane Note 1 to entry: Graphene oxide is a single-layer material with a high oxygen content, typically characterized by O/C atomic ratios of approximately 0,5 depending on the method of synthesis. [SOURCE: ISO 80004-13:2024, 3.1.2.13]
4 Abbreviated terms
A flake area AFM atomic force microscopy Cl compactness relative to the major axis length of the equivalent ellipse ECD equivalent circular diameter GO graphene oxide H difference in maximum frequency height values L major axis length of equivalent ellipse maj L minor axis length of equivalent ellipse min LR ratio of major axis to minor axis lengths SE secondary electron SEM scanning electron microscopy 2D two-dimensional x maximum frequency height value of substrate by Gaussian fit c1 x maximum frequency height value of sample by Gaussian fit c2
5 Overview
This document provides methods to measure the lateral size and thickness of GO flakes in a powder or liquid dispersion form. If confirmation of the presence of GO is required, use the methods detailed in ISO/TS 21356-1 and ISO/TS 23356.
ISO/DTS 23879:2026(en) Follow the sequence of methods as detailed in Figure 1 to determine the lateral size and thickness of GO flakes. Use SEM to measure the lateral size of GO oxide flakes as detailed in Clause 7 and then use AFM to determine thickness as detailed in Clause 8. Whilst using SEM allows the measurement of the lateral size of a statistically relevant number of flakes, it cannot be used to measure the thickness. Conversely, AFM can be used to measure both the lateral size and thickness, although it cannot currently be used to provide the same statistically relevant data in the same timeframe.
NOTE The numbers in brackets are the respective clauses.
Figure 1 — Overview of the sequence of the measurement methods used to determine the lateral size and thickness of GO flakes
6 Sample preparation
For both SEM and AFM analysis, GO liquid dispersion should be deposited onto a clean substrate such that there is then good separation between individual GO flakes as detailed below. A clean substrate can be obtained e.g. via sonication in ethanol and, subsequently, in isopropyl alcohol, for 10 min for each solvent, ozone cleaned for 30 min and dried with N gas in between each step and at the end of the whole cleaning
process. Samples for SEM should be produced using a clean silicon wafer with a minimal oxide layer (ideally native but up to 90 nm), whilst AFM samples should be produced using a freshly cleaved mica surface. The following are the sample preparation steps:
a) Powder samples shall first be dispersed in an appropriate solvent to form a liquid dispersion before deposition onto the surface. For pure GO, water is a good suspension medium. If the powder does not readily disperse, then ethanol can also be added. Figure 2 (right) shows the result of deposition from a [11] mix of demineralized and deionized water with isopropyl alcohol in equal volumes. b) A concentration of 0,05 mg/mL for the dispersion of GO flakes is recommended in a tube to be mixed using low-shear dispersion methods (e.g. gentle stirring or orbital shaking). Where possible, ultrasonication should be avoided for GO dispersion. Even short exposures (e.g. ≤40 s at ≈100 W) can induce sheet breakage and bias the measured flake-size distribution. However, if, in exceptional cases, ultrasonication is required, parameters should be minimized and if possible validated to show that no measurable change in the size distribution (e.g. pre-/post-sonication ECD statistics) occur. c) Then, the upper mixture is further diluted 5 to 10 times to obtain the isolated flakes, see Figure 2 (a). d) Dip-coating 6 µL of the dispersion onto the clean substrate (1 cm × 1 cm) to obtain uniform deposits, showing reduced coffee-ring effects.
Alternatively to the dip-coating procedure, drop-casting can be carried out, see Figure 2 (b), where a [11] droplet of 10 μL solution was deposited on the SiO /Si substrate. More details are given in B.2.
e) Air-dry the samples at room temperature for at least 20 minutes. Prepare the samples in a clean environment, for example in a cleanroom, or glass petri dishes. The sample can then be analysed. Following preparation, the samples retain stability for up to six months through storage in vacuumsealed container or aluminum foil packaging.
ISO/DTS 23879:2026(en) NOTE 1 Item a) shows isolated flakes (best scenario).
NOTE 2 Item b) mark flakes whose boundaries are slightly touching each other but where the border of the flakes is still clearly distinguishable.
NOTE 3 Item c) marks overlapping flakes not suitable for measurement. Figure 2 — Suitable and unsuitable flakes for measurement
7 Scanning electron microscopy
7.1 General
SEM works by scanning the sample surface with an electron beam and analysing the electrons after interaction with the material. Based on the analysis of this information, the two-dimensional surface morphology of the sample can be obtained.
7.2 Imaging
Use a field-emission SEM that is dimensionally calibrated using traceable dimensional calibration standards. The calibration should be valid for the working distance and accelerating voltage used in the subsequent measurements. A field-emission SEM equipped with a secondary electron detector with resolution better than 10 nm is recommended. A secondary electron in lens detector is preferred over the conventional Everhart-Thornley (ET) detector in order to provide superior contrast and sharper flake edges. Mount the sample firmly in the SEM holder so that it is held rigidly in place in the chamber. Pump down to vacuum. When the vacuum of SEM is suitable for operation, select an appropriate accelerating voltage of 3 kV or less to minimize charging. The SEM should be operated at the lowest acceleration voltage possible where the contrast of the image still gives a clear definition of the GO flake boundary from the background that is compatible with image processing. The image brightness and contrast shall be adjusted such that the grayscale value of the GO flakes obtained in the SEM image is significantly different to that of the substrate, and with clear boundaries of the GO flakes.
Identify a region of interest and then optimise the image by adjusting the aperture, working distance, stigmator and focus, to achieve the best resolution possible. This process should be carried out on a flake that will not be subsequently used for measurement. Low magnification images (~10 k magnification) should then be obtained for areas that contain flakes to ensure that the region is suitable. Then, images of greater magnification should be obtained for the flakes such that the whole flake is in the field of view. The magnification and pixel size should be adapted to the size of the flake. In case that the morphology of the whole flake is clearly captured, a greater magnification and a smaller pixel size are recommended to reduce measurement uncertainty.
A representative distribution of flakes with different sizes from across the substrate surface shall be imaged. Repeat the SEM measurements for different areas of the substrate until more than 200 randomly chosen
ISO/DTS 23879:2026(en) flakes have been imaged and are suitable for analysis. If greater precision is required, then a higher number of flakes can be analysed.
Suitable flakes for measurement are:
a) isolated flakes (best scenario); b) flakes whose boundaries are slightly touching each other but where the border of the flakes is still clearly distinguishable (this can be easily obtained using the SE in lens detector); c) overlapped flakes where the border of the flakes is still clearly distinguishable (this can be easily obtained using the SE in lens detector) as shown in Figure 2.
Flakes that are not suitable for measurement are:
- flake clusters where the overlapping flakes are so numerous that their boundaries cannot be distinguished anymore;
- bulky graphitic particles;
- folded flakes (with substantial folded areas).
The largest source of bias in the measurement of the average lateral flake size is typically flake selection, rather than the limits on the instrument itself. Thus, it is extremely important that the user does not preferentially measure flakes of specific shapes or sizes, but rather analyses all flakes that are possible in each image. ISO 19749 provides a general reference of guidance for measuring size and shape distribution of nanoparticles including general principles, sample preparation, qualification of the SEM, image acquisition, particle and data analysis.
NOTE Example operating conditions are an accelerating voltage of 3 kV, working distance of <4 mm and magnification of 3 000× and low beam current (< 1 nA). Image capture frame time of 20 s.
7.3 Data analysis
7.3.1 Image analysis method and required parameters
Use appropriate imaging software to analyse the images. Care should be taken to set the scale correctly. Measure the flake size of at least 200 flakes using one or both of the two approaches detailed below. The largest source of bias in the measurement of the average lateral flake size is typically due to flake selection, rather than the limits on the instrument itself or choice of the methods below. Thus, it is extremely important that the user does not preferentially measure flakes of specific shapes or sizes, but rather analyses all flakes that are possible in each image.
The lateral size of each flake should be determined by measuring the length and then the width of each flake. There are various size descriptors to characterize the length and width of an object, e. g.:
a) simply length and width; b) minimum Feret and maximum Feret; c) major and minor axes of the equivalent ellipse; d) the equivalent circular diameter (ECD), which is the diameter of a circle with the same area as the object. Figure 3 shows possible ways to determine these parameters. When reporting the lateral size values, the type of analysis should be described.
ISO/DTS 23879:2026(en) Input: → Output Input: → Output Manual Area, perimeter Length ECD contouring Feret ratio Width Aspect (F /F ) ECD ratio min max a) Minimum Feret and maximum Feret b) Minimum width and maximum length Key 1 maxFeret 2 minFeret 3 length 4 width Input: → Output Input: → Output Automated ECD Automated ECD contouring LR contouring Cl c) Minor axis length and major axis length of equiva- d) Diameter of a circle with the same area as lent ellipse the object NOTE The characterization descriptors for lateral size and shape of GO flakes using SEM are reported in Annex A. Figure 3 — Example image analysis results showing four possible image analysis approaches used to analyse the same flakes
7.3.2 Approach 1: Perimeter tracing
For this approach, the boundary or perimeter of each GO flake should be manually traced (contoured) by the operator using appropriate software tools or the flakes can be automatically contoured using an appropriate method. The steps for this can include image binarization, Gaussian filtering, image grey adjustment, region segmentation. Annex B details examples of both methods. From the contoured areas, the size descriptors:
area, perimeter, minFeret, maxFeret, minor axis length and major axis length, ECD should be extracted for each flake.
ISO/DTS 23879:2026(en)
...
Contents
- Introduction
- 1 Scope
- 2 Normative references
- 3 Terms and definitions
- 4 Abbreviated terms
- 5 Overview
- 6 Sample preparation
- 7 Scanning electron microscopy
- 7.1 Introduction
- 7.1 General
- 7.2 Imaging
- 7.3 Data analysis
- 8 Atomic force microscopy
- 8.1 Introduction
- 8.1 General
- 8.2 Method
- 8.3 Image and data analysis to obtain flake height
- 9 Reporting
- Annex A
- Annex B
- Annex C
- Annex D
- 1 Name of Operator
- 2 Sample Description
- 3 Instrument name/details
- 4. Instrument calibration details (sample, date, etc)
- 5. Instrument imaging descriptors
- 6. Data analysis
- 7. Data Recording(recording (see Table D.1Table D.1 and Table D.2Table D.2))
- Bibliography
Introduction
Graphene oxide (GO) is an oxidized form of graphene functionalised with oxygen-containing groups. It is a single layer two-dimensional material with an oxygen-to-carbon ratio of approximately 0,5, which is prepared by oxidation and exfoliation of graphite, causing extensive oxidative modification of the basal plane. The benefits of this material have been shown for many fields such as catalysts, supercapacitors, Li-ion batteries, [1] [1-4] ]-[ [4] nanofluids and composites. . GO flakes come in many different sizes and shapes, thus when GO is [5] [5],[ 6] ],[ [6] incorporated into a macroscopic material, these differences affect the material’s properties. . For example, lateral flake size has a significant influence on mechanical properties and corrosion protection when [7] [7]-[10] ]-[ [10] GO is used in composite materials. .
Scanning electron microscopy (SEM) is a key technique for the visualization of GO flakes and measurement of their lateral sizes. The sample pre-treatment, the collection of micrographs and the procedures for the image analysis require a standardized method to ensure the consistency and reliability of reported material properties.
Atomic force microscopy (AFM) is a powerful technique for the measurement of features at the nanoscale. For GO, this includes flake thickness and lateral size. However, although the theoretical value of single-layer GO is known, in reality measurement uncertainties due to contaminants and instrument noise can be large, such that the thickness can not be accurately measured by common data processing methods. Therefore, it is highly desirable to standardize a method to ensure the consistency and reliability of measurement results. This document describes the methodology for measuring the lateral size and thickness of GO flakes using SEM and AFM, respectively. It aims to provide a reliable measurement methodology for determining GO lateral size and thickness, that can be used by the GO supply chain.
ISO/DTS 23879:2026(E:(en) Nanotechnologies – — Structural characterization of graphene oxide flakes: — Thickness and lateral size and thickness measurement using SEMatomic force microscopy and AFMscanning electron microscopy
1 Scope
This document describes methods for measuring the lateral size and thickness of graphene oxide (GO) flakes using scanning electron microscopy (SEM) and atomic force microscopy (AFM), respectively, including sample pre-treatments, collection of micrographs and data analysis. It is applicable to the characterization of GO in powder and liquid dispersion forms.
2 Normative references
The following documents are referred to in the text in such a way that some or all of their content constitute requirements of this document. For dated references, only the edition cited applies. For undated references, the latest edition of the referenced document (including any amendments) applies. ISO 18115-2, Surface chemical analysis — Vocabulary — Part 2: Terms used in scanning-probe microscopy ISO/TS 80004-13, Nanotechnologies — Vocabulary — Part 13: Graphene and relatedother two-dimensional (2D) materials
3 Terms and definitions
For the purposes of this document, the terms and definitions given in ISO 18115-2:2010 and ISO/TS 80004- 13:2017 and the following apply.
ISO and IEC maintain terminology databases for use in standardization at the following addresses:
- — ISO Online browsing platform: available at https://www.iso.org/obp
- — IEC Electropedia: available at https://www.electropedia.org/ 3.1 3.1 atomic force microscopy AFM method for imaging surfaces by mechanically scanning their surface contours, in which the deflection of a sharp tip sensing the surface forces, mounted on a compliant cantilever, is monitored Note 1 to entry: AFM can provide a quantitative height image of both insulating and conducting surfaces. Note 2 to entry: Some AFM instruments move the sample in the x-, y- and z-directions while keeping the tip position constant and others move the tip while keeping the sample position constant. Note 3 to entry: AFM can be conducted in vacuum, a liquid, a controlled atmosphere or air. Atomic resolution may be attainable with suitable samples, with sharp tips and by using an appropriate imaging mode. Note 4 to entry: Many types of force can be measured, such as the normal forces or the lateral, friction or shear force. When the latter is measured, the technique is referred to as lateral, frictional or shear force microscopy. This generic term encompasses all of these types of force microscopy.
ISO/DTS 23879:2026(E:(en) Note 5 to entry: AFMs can be used to measure surface-normal forces at individual points in the pixel array used for imaging.
Note 6 to entry: For typical AFM tips with radii < 100 nm, the normal force should be less than about 0,1 μN, depending on the sample material, or irreversible surface deformation, and excessive tip wear occurs. [SOURCE: ISO 18115-2:2013, 3.2] 3.2 3.2 scanning electron microscopy SEM method that examines and analyses the physical information (such as secondary electrons, backscattered electrons, absorbed electrons and x-ray radiation) obtained by generating electron beams and scanning the surface of the sample in order to determine the structure, composition and topography of the sample [SOURCE: ISO 80004-6:2021, 4.5.5 ] 3.3 3.3 graphene oxide GO chemically modified graphene prepared by oxidation and exfoliation of graphite, causing extensive oxidative modification of the basal plane Note 1 to entry: Graphene oxide is a single-layer material with a high oxygen content, typically characterized by O/C atomic ratios of approximately 0,5 depending on the method of synthesis. [SOURCE: ISO 80004-13:2024, 3.1.2.13]
4 Abbreviated terms
A flake area AFM atomic force microscopy Cl compactness relative to the major axis length of the equivalent ellipse ECD equivalent circular diameter GO graphene oxide H difference in maximum frequency height values L major axis length of equivalent ellipse maj L minor axis length of equivalent ellipse min LR ratio of major axis to minor axis lengths SE secondary electron SEM scanning electron microscopy 2D two-dimensional x maximum frequency height value of substrate by Gaussian fit c1 x maximum frequency height value of sample by Gaussian fit c2
ISO/DTS 23879:2026(E:(en)
5 Overview
This document provides methods to measure the lateral size and thickness of GO flakes in a powder or liquid dispersion form. If confirmation of the presence of GO is required, use the methods detailed in ISO/TS 21356- 1 and ISO/TS 23356.
Follow the sequence of methods as detailed in Figure 1Figure 1 to determine the lateral size and thickness of GO flakes. Use SEM to measure the lateral size of GO oxide flakes as detailed in Clause 7clause 7 and then use AFM to determine thickness as detailed in Clause 8clause 8.. Whilst using SEM allows the measurement of the lateral size of a statistically relevant number of flakes, it cannot be used to measure the thickness. Conversely, AFM can be used to measure both the lateral size and thickness, although it cannot currently be used to provide the same statistically relevant data in the same timeframe.
Note:
NOTE The numbers in brackets are the respective clauses.
Figure 1 — Overview of the sequence of the measurement methods used to determine the lateral size and thickness of GO flakes.
6 Sample preparation
For both SEM and AFM analysis, GO liquid dispersion should be deposited onto a clean substrate such that there is then good separation between individual GO flakes as detailed below. A clean substrate can be obtained e.g. via sonication in ethanol and, subsequently, in isopropyl alcohol, for 10 min for each solvent, ozone cleaned for 30 min and dried with N gas in between each step and at the end of the whole cleaning
process. Samples for SEM should be produced using a clean silicon wafer with a minimal oxide layer (ideally native but up to 90 nm), whilst AFM samples should be produced using a freshly cleaved mica surface. The following are the sample preparation steps:
a) 1) Powder samples shall first be dispersed in an appropriate solvent to form a liquid dispersion before deposition onto the surface. For pure GO, water is a good suspension medium. If the powder does not readily disperse, then ethanol can also be added. Figure 2Figure 2 (right) shows the result of deposition [11] [11] from a mix of demineralized and deionized water with isopropyl alcohol in equal volumes. .
ISO/DTS 23879:2026(E:(en) b) 2) A concentration of 0.,05 mg/mL for the dispersion of GO flakes is recommended in a tube to be mixed using low-shear dispersion methods (e.g. gentle stirring or orbital shaking). Where possible, ultrasonication should be avoided for GO dispersion. Even short exposures (e.g. ≤40 s at ≈100 W) can induce sheet breakage and bias the measured flake-size distribution. However, if, in exceptional cases, ultrasonication is required, parameters should be minimized and if possible validated to show that no measurable change in the size distribution (e.g. pre-/post-sonication ECD statistics) occur. c) 3) Then, the upper mixture is further diluted 5 to 10 times to obtain the isolated flakes, see Figure 2Figure 2 (a).
d) 4) Dip-coating 6 µL of the dispersion onto the clean substrate (1 cm × × 1 cm) to obtain uniform deposits, showing reduced coffee-ring effects.
Alternatively to the dip-coating procedure, drop-casting can be carried out, see Figure 2Figure 2 (b), [11] [11] where a droplet of 10 μL solution was deposited on the SiO /Si substrate. . More details are given in
B.2B.2..
e) 5) Air-dry the samples at room temperature for at least 20 minutes. Prepare the samples in a clean environment, for example in a cleanroom, or glass petri dishes. The sample can then be analysed. Following preparation, the samples retain stability for up to six months through storage in vacuum-sealed container or aluminum foil packaging.
Note NOTE 1: Item a) shows isolated flakes (best scenario)).
NoteNOTE 2: Item b) mark flakes whose boundaries are slightly touching each other but where the border of the flakes is still clearly distinguishable.
NoteNOTE 3: Item c) marks overlapping flakes not suitable for measurement .
ISO/DTS 23879:2026(E:(en) Figure 2 — Suitable and unsuitable flakes for measurement.
ISO/DTS 23879:2026(E:(en)
7 Scanning electron microscopy
7.1 Introduction
7.1 General
SEM works by scanning the sample surface with an electron beam and analysing the electrons after interaction with the material. Based on the analysis of this information, the two-dimensional surface morphology of the sample can be obtained.
7.2 Imaging
Use a field-emission SEM that is dimensionally calibrated using traceable dimensional calibration standards. The calibration should be valid for the working distance and accelerating voltage used in the subsequent measurements. A field-emission SEM equipped with a secondary electron detector with resolution better than 10 nm is recommended. A secondary electron in lens detector is preferred over the conventional Everhart- Thornley (ET) detector in order to provide superior contrast and sharper flake edges. Mount the sample firmly in the SEM holder so that it is held rigidly in place in the chamber. Pump down to vacuum. When the vacuum of SEM is suitable for operation, select an appropriate accelerating voltage of 3 kV or less to minimize charging. The SEM should be operated at the lowest acceleration voltage possible where the contrast of the image still gives a clear definition of the GO flake boundary from the background that is compatible with image processing. The image brightness and contrast shall be adjusted such that the grayscale value of the GO flakes obtained in the SEM image is significantly different to that of the substrate, and with clear boundaries of the GO flakes.
Identify a region of interest and then optimise the image by adjusting the aperture, working distance, stigmator and focus, to achieve the best resolution possible. This process should be carried out on a flake that will not be subsequently used for measurement. Low magnification images (~10k10 k magnification) should then be obtained for areas that contain flakes to ensure that the region is suitable. Then, images of greater magnification should be obtained for the flakes such that the whole flake is in the field of view. The magnification and pixel size should be adapted to the size of the flake. In case that the morphology of the whole flake is clearly captured, a greater magnification and a smaller pixel size are recommended to reduce measurement uncertainty.
A representative distribution of flakes with different sizes from across the substrate surface shall be imaged. Repeat the SEM measurements for different areas of the substrate until more than 200 randomly chosen flakes have been imaged and are suitable for analysis. If greater precision is required, then a higher number of flakes can be analysed.
Suitable flakes for measurement are 1) :
a) isolated flakes (best scenario), 2) ); b) flakes whose boundaries are slightly touching each other but where the border of the flakes is still clearly distinguishable (this can be easily obtained using the SE in lens detector) 3) ); a)c) overlapped flakes where the border of the flakes is still clearly distinguishable (this can be easily obtained using the SE in lens detector) as shown in Figure 2Figure 2. . Flakes that are not suitable for measurement are: 1) - flake clusters where the overlapping flakes are so numerous that their boundaries cannot be distinguished anymore, 2) ;
ISO/DTS 23879:2026(E:(en) - bulky graphitic particles 3) ; - folded flakes (with substantial folded areas).
The largest source of bias in the measurement of the average lateral flake size is typically flake selection, rather than the limits on the instrument itself. Thus, it is extremely important that the user does not preferentially measure flakes of specific shapes or sizes, but rather analyses all flakes that are possible in each image. ISO 19749 provides a general reference of guidance for measuring size and shape distribution of nanoparticles including general principles, sample preparation, qualification of the SEM, image acquisition, particle and data analysis.
NOTE Example operating conditions are an accelerating voltage of 3 kV, working distance of <4 mm and magnification of 30003 000× and low beam current (< 1 nA). Image capture frame time of 20 s.
7.3 Data analysis
7.3.1 Image analysis method and required parameters
Use appropriate imaging software to analyse the images. Care should be taken to set the scale correctly. Measure the flake size of at least 200 flakes using one or both of the two approaches detailed below. The largest source of bias in the measurement of the average lateral flake size is typically due to flake selection, rather than the limits on the instrument itself or choice of the methods below. Thus, it is extremely important that the user does not preferentially measure flakes of specific shapes or sizes, but rather analyses all flakes that are possible in each image.
The lateral size of each flake should be determined by measuring the length and then the width of each flake. There are various size descriptors to characterize the length and width of an object, e. g. a) .:
a) simply length and width, b) ; b) minimum Feret and maximum Feret, c) ; c) major and minor axes of the equivalent ellipse, or d) ; d) the equivalent circular diameter (ECD), which is the diameter of a circle with the same area as the object. Figure 3 Figure 3 shows possible ways to determine these parameters. When reporting the lateral size values, the type of analysis should be described.
a) b) Input: Output Input: Output Manual Area, perimeter Length ECD
ISO/DTS 23879:2026(E:(en) contouring Feret Ratio (Fmin/Fmax) Width Aspect Ratio ECD
a) minimum Feret and maximum Feret b) minimum width and maximum length
Key 1 maxFeret 3 length 2 minFeret 4 width
c) d) Input: Output Input: Output Automated ECD Automated ECD contouring LR contouring Cl c) minor axis length and major axis length of equivalent ellipse d) diameter of a circle with the same area as the object
Note :
Input: → Output Input: → Output Manual Area, perimeter Length ECD contouring Feret ratio Width Aspect ratio (Fmin/Fmax) ECD a) Minimum Feret and maximum Feret b) Minimum width and maximum length Key 1 maxFeret 2 minFeret 3 length 4 width
ISO/DTS 23879:2026(E:(en)
Input: → Output Input: → Output Automated ECD Automated ECD contouring LR contouring Cl c) Minor axis length and major axis length of equivalent ellipse d) Diameter of a circle with the same area as the object NOTE The characterization descriptors for lateral size and shape of GO flakes using SEM are reported in Annex AAnnex A.
Figure 3 — Example image analysis results showing four possible image analysis approaches used to analyse the same flakes
7.3.2 Approach 1: Perimeter tracing
For this approach, the boundary or perimeter of each GO flake should be manually traced (contoured) by the operator using appropriate software tools or the flakes can be automatically contoured using an appropriate method. The steps for this can include image binarization, Gaussian filtering, image grey adjustment, region segmentation. Annex BAnnex B details examples of both methods. From the contoured areas, the size descriptors: area, perimeter, minFeret, maxFeret, minor axis length and major axis length, ECD should be extracted for each flake.
7.3.3 7.3.3 Approach 2: Length and width via perpendicular bisector The dimensions of each flake are determined by measuring the length and then the width of the flake. The length and width of the flake shall be defined so that they would approximately be the length and width of the flake within the smallest rectangle or ellipse that best represent the particle shape. Both the length and width segments should fall within the boundaries of the particle.
...