Abstract

This document details the methods for characterising the structural properties of CVD-grown graphene. The methods used are optical microscopy, Raman spectroscopy and transmission electron microscopy (TEM). The properties determined are the percentage of substrate coverage of graphene, number of layers, the level of disorder and layer stacking. Sample preparation routines, measurement protocols and data analysis for the characterisation of CVD-grown graphene are provided.

Status
Not Published
Technical Committee
ISO/TC 229 - Nanotechnologies
Current Stage
6000 - International Standard under publication - 60 Publication
Start Date
26-Aug-2026

Buy Documents

Draft

ISO/DTS 21356-2 - Nanotechnologies — Structural characterization of graphene — Part 2: Graphene sheets on a substrate

Release Date:19-May-2026
English language (34 pages)
sale 15% off
sale 15% off
Draft

REDLINE ISO/DTS 21356-2 - Nanotechnologies — Structural characterization of graphene — Part 2: Graphene sheets on a substrate

Release Date:19-May-2026
English language (34 pages)
sale 15% off
sale 15% off

ISO/TS 21356-2 is an ISO technical specification for the structural characterization of graphene sheets on a substrate. It specifies a step-by-step way to prepare transferred graphene and measure substrate coverage, number of layers, disorder, and layer stacking using optical microscopy, Raman spectroscopy, TEM and SAED. It is aimed at laboratories, manufacturers and inspectors who need comparable results for CVD-grown graphene sheets and other graphene sheets that can be transferred to suitable substrates.

What does ISO/TS 21356-2 specify?

ISO/TS 21356-2 specifies methods for characterizing graphene sheets on a substrate, mainly CVD-grown graphene and graphene sheets made by alternative methods if they can be transferred to the required supports. The document focuses on structural characterization, not on graphene supplied as powders or liquid dispersions.

The scope covers sample preparation, measurement protocols and data analysis for four measurands - percentage substrate coverage, number of layers, level of disorder and layer stacking. The document is organized into clauses for scope, references, terms, abbreviations, the measurement sequence, sample transfer and preparation, optical microscopy, Raman spectroscopy, TEM and SAED, and reporting. Two informative annexes summarize interlaboratory studies that support the Raman and TEM/SAED methods.

AnnexWhat it covers
Annex ASummary of a Raman spectroscopy interlaboratory study
Annex BSummary of a TEM/SAED interlaboratory study

What are the key requirements of ISO/TS 21356-2?

ISO/TS 21356-2 requires a defined sequence of measurements because each method answers a different part of the characterization. In practice, the user first prepares the right substrate for optical microscopy and Raman spectroscopy, then transfers a separate part of the same sheet to a TEM grid for TEM and SAED.

Sample transfer and preparation

Clause 6 gives transfer routes for graphene on copper and for graphene already on Si/SiO2. For copper-grown CVD graphene, the document uses PMMA support, oxygen plasma on the back side, ammonium persulphate etching, and repeated DI water rinses. For TEM from Si/SiO2, it uses PMMA support, baking, KOH etching, DI water rinsing and transfer to a TEM grid.

For optical microscopy and Raman spectroscopy, the graphene sheet is placed on a silicon wafer with a SiO2 thickness of either 90 nm or 300 nm. The wafer is cleaned, dried and checked for particles or residue. This matters because the contrast needed to see graphene depends strongly on the substrate, and contamination can affect both visibility and later analysis.

Optical microscopy first for coverage screening

Clause 7 uses optical microscopy to estimate how much of the substrate is covered by graphene. The method calls for an objective of 20x or higher and uses the selected sample positions to give a representative coverage map across the substrate or the transferred sheet.

The optical result is split into no graphene, 1LG, and areas with more than one layer. If the sheet is discontinuous, the document distinguishes islands from holes. This gives a fast first pass on transfer quality and coverage, and it helps decide where Raman and TEM should focus.

Raman spectroscopy for coverage, layer count and disorder

Clause 8 specifies Raman spectroscopy in a 180 degree backscattering geometry with a 50x or 100x objective and NA at least 0.75. A 532 nm laser is preferred on Si/SiO2, with 514 nm allowed if needed, and the incident laser power must stay below 1 mW. These limits matter because they reduce heating and make spectra more comparable.

The Raman mapping protocol uses at least a 10 µm x 10 µm map with 121 spectra and repeated maps across the sample. The document then fits the D, G and 2D peaks, using a pseudo-Voigt function after baseline subtraction. From these fits, it derives the G-peak area, intensity ratios such as I2D/IG and ID/IG, and the FWHM of the G and 2D peaks.

The document uses these Raman results to separate 1LG from 2LG and FLG, and to estimate disorder. In practice, the user needs to record the laser wavelength, power, calibration method, temperature, humidity and all map results because the layer assignment depends on these settings and on the fitted peak shape.

TEM and SAED to confirm stacking and fine structure

Clause 9 uses TEM and SAED to confirm the number of layers, layer alignment and defects. The method calls for a modern TEM or STEM instrument, with 80 kV used for imaging and low electron flux to limit damage. Sample baking before loading is used to reduce contamination, which matters because residues can obscure atomic contrast and change the diffraction pattern.

SAED uses a small selected area aperture, and the document analyzes the ratio of the second-order to first-order diffraction spots to distinguish 1LG from 2LG and thicker material. The same section also distinguishes Bernal stacking from turbostratic stacking and uses HRTEM to record defect types such as edges, grain boundaries and point defects. This is the method that provides the strongest confirmation when Raman alone is ambiguous.

Reporting and traceability

Clause 10 requires reporting of sample history, transfer route, substrate details, calibration, measurement settings and the main results. For Raman, the report includes the peak-processing method, map data and the calculated coverage and disorder values. For TEM, the report includes the accelerating voltage, flux, fluence, SAED aperture size, camera length, acquisition time, stacking observations and defect observations.

What terms does ISO/TS 21356-2 define?

  • 1LG - single layer graphene, also called monolayer graphene, meaning one graphene layer made of carbon atoms in a honeycomb structure.
  • 2LG - bilayer graphene, meaning two well-defined stacked graphene layers.
  • FLG - few-layer graphene, meaning graphene with three to ten well-defined stacked layers.
  • Bernal stacking - a stacking arrangement where neighboring layers are offset so that only half of the atoms line up in the out-of-plane direction.
  • turbostratic stacking - a stacking arrangement with relative rotational misalignment between layers, not described as Bernal or rhombohedral stacking.
  • sheet - a 2D material typically located on a substrate with extended lateral dimensions.
  • Raman shift - the energy difference between the incident and scattered photon in Raman spectroscopy, usually reported in wavenumbers.

Who uses ISO/TS 21356-2?

ISO/TS 21356-2 is used by laboratories that inspect CVD-grown graphene sheets, by manufacturers and process engineers working with transferred graphene, and by quality teams that need a repeatable way to compare samples. It is also relevant to metrology institutes, universities and instrument manufacturers, which are identified in the interlaboratory work cited in the document.

In practice, users apply it when they need to check whether a graphene sheet is continuous, how much of a substrate it covers, whether it is mostly 1LG or contains 2LG/FLG, and whether the layer stacking is Bernal or turbostratic. It is useful wherever graphene transfer quality, layer count or disorder need to be documented in a consistent way.

Which standards are used with ISO/TS 21356-2?

StandardWhat it contributes
ISO/TS 80004-1Core nanotechnology terms
ISO/TS 80004-6Vocabulary for nano-object characterization
ISO/TS 80004-13Vocabulary for graphene and other 2D materials, including graphene-layer terms and stacking terms
ISO 21363TEM guidance for particle size and shape distributions, and supporting practice for TEM image formation and diffraction
ISO/TS 21356-1The companion part for graphene from powders and dispersions

What does the ISO/TS 21356-2 document contain?

ISO/TS 21356-2 contains a flow chart for the measurement sequence, sample transfer procedures, optical microscopy mapping guidance, Raman peak-fitting and map-analysis methods, and TEM/SAED acquisition and analysis steps. It also contains reporting checklists and example figures that show how to recognize coverage patterns, peak shapes, diffraction patterns and defect cases.

The informative annexes summarize interlaboratory studies for Raman spectroscopy and for TEM/SAED. Those annexes support method selection and give users context for why the document uses specific fitting and analysis choices.

Buy Documents

Draft

ISO/DTS 21356-2 - Nanotechnologies — Structural characterization of graphene — Part 2: Graphene sheets on a substrate

Release Date:19-May-2026
English language (34 pages)
sale 15% off
sale 15% off
Draft

REDLINE ISO/DTS 21356-2 - Nanotechnologies — Structural characterization of graphene — Part 2: Graphene sheets on a substrate

Release Date:19-May-2026
English language (34 pages)
sale 15% off
sale 15% off

Frequently Asked Questions

ISO/TS 21356-2 is a draft published by the International Organization for Standardization (ISO). Its full title is "Nanotechnologies — Structural characterization of graphene — Part 2: Graphene sheets on a substrate". This standard covers: This document details the methods for characterising the structural properties of CVD-grown graphene. The methods used are optical microscopy, Raman spectroscopy and transmission electron microscopy (TEM). The properties determined are the percentage of substrate coverage of graphene, number of layers, the level of disorder and layer stacking. Sample preparation routines, measurement protocols and data analysis for the characterisation of CVD-grown graphene are provided.

This document details the methods for characterising the structural properties of CVD-grown graphene. The methods used are optical microscopy, Raman spectroscopy and transmission electron microscopy (TEM). The properties determined are the percentage of substrate coverage of graphene, number of layers, the level of disorder and layer stacking. Sample preparation routines, measurement protocols and data analysis for the characterisation of CVD-grown graphene are provided.

ISO/TS 21356-2 is classified under the following ICS (International Classification for Standards) categories: 07.120 - Nanotechnologies. The ICS classification helps identify the subject area and facilitates finding related standards.

ISO/TS 21356-2 is available in PDF format for immediate download after purchase. The document can be added to your cart and obtained through the secure checkout process. Digital delivery ensures instant access to the complete standard document.

Standards Content (Sample)

Contents

  • Introduction
  • 1 Scope
  • 2 Normative references
  • 3 Terms and definitions
  • 3.1 graphene
  • 3.2 graphite
  • 3.3 bilayer graphene
  • 3.4 few-layer graphene
  • 3.5 Bernal stacking
  • 3.6 stacking angle
  • 3.7 turbostratic stacking
  • 3.8 defect
  • 3.9 sheet
  • 3.10 Raman spectroscopy
  • 3.11 Raman shift
  • 4 Abbreviated terms
  • 5 Sequence of measurement methods
  • 6 Sample transfer and preparation
  • 6.1 Introduction
  • 6.2 Removal from copper substrate
  • 6.3 Removal from silicon dioxide on silicon substrate
  • 6.4 Silicon wafer substrate preparation
  • 6.5 Sample and substrate preparation and transfer
  • 7 Determination of coverage of graphene using optical microscopy
  • 7.1 Introduction
  • 7.2 Measurement protocol
  • 7.3 Data analysis
  • 8 Raman spectroscopy of a graphene sheet
  • 8.1 Introduction
  • 8.2 Instrumentation
  • 8.3 Measurement method
  • 8.4 Curve fitting
  • 8.5 Determination of graphene properties
  • 8.6 Reporting
  • 9 TEM and SAED of a graphene sheet
  • 9.1 Introduction
  • 9.2 Instrumentation
  • 9.3 Measurement protocol
  • 9.4 Data analysis
  • 1 TEM image from a contaminated sample
  • 2 SAED pattern from a contaminated sample
  • 3 TEM image from a torn sample
  • 4 SAED pattern from a torn sample
  • 5 TEM image from a creased sample
  • 6 SAED pattern from a creased sample
  • 7 TEM image from a sample with grain boundaries
  • 8 SAED pattern from a sample with grain boundaries
  • 10 Reporting
  • 10.1 General
  • 10.2 Sample preparation
  • 10.3 Raman spectroscopy
  • 10.4 TEM
  • Annex A
  • Annex B
  • Bibliography

Introduction

Graphene is starting to impact many different application areas such as solar cells, biosensors, displays, composites, flexible electronics and energy storage due to its exceptional properties. As industry uptake of this material increases, international standardization is critical to enable commercialization. Reliable, accurate, and reproducible measurements are important due to many production routes and producers of the material, in order to enable comparability and maintain high quality manufacture. There are, in general, two forms of commercially-available graphene, namely flakes/particles or a sheet on a substrate. The former are supplied in the form of a powder or liquid dispersion and can be flake-like in nature but can vary in lateral size and thickness, thus commercial-available material is also likely to contain thicker flakes classed as graphite. The structural characterization of these materials is described in ISO/TS 21356-1:2021,Nanotechnologies — Structural characterization of graphene —Part 1: Graphene from powders and dispersions.

This document, the second part of the ISO/TS 21356 series, describes the structural characterization of graphene in the form of a sheet, predominantly produced via chemical vapour deposition (CVD), but applicable to graphene sheets produced using alternative methods, that can be transferred onto appropriate substrates. It provides a flow-chart for analysts to follow. It details the methods for characterizing the structural properties of graphene sheets in a systematic way. The methods used are optical microscopy, Raman spectroscopy and transmission electron microscopy (TEM). Note that graphene related twodimensional materials deposited onto substates as particles from powders or liquid dispersions are not addressed in this document, but are addressed within ISO/TS 21356-1,Nanotechnologies — Structural characterization of graphene. Part 1: Graphene from powders and dispersions. The measurands determined are:

a) the percentage of substrate covered by graphene; b) the number of layers; c) the level of disorder; d) the layer stacking.

For each technique, sample preparation routines, measurement protocols and ways to analyze the data are provided.

FINAL DRAFT Technical Specification ISO/DTS 21356-2:2026(en) Nanotechnologies — Structural characterization of graphene — Part 2:

Graphene sheets on a substrate

1 Scope

This document details the methods for characterizing the structural properties of CVD-grown graphene, or graphene sheets produced using alternative methods, which can be transferred onto appropriate substrates. The methods used are optical microscopy, Raman spectroscopy, transmission electron microscopy (TEM) and selected area electron diffraction (SAED). The properties determined are the percentage of substrate covered by graphene, the number of layers, the level of disorder and the layer stacking. Sample preparation routines, measurement protocols and data analysis for the characterization of graphene sheets are provided.

2 Normative references

The following documents are referred to in the text in such a way that some or all of their content constitutes requirements of this document. For dated references, only the edition cited applies. For undated references, the latest edition of the referenced document (including any amendments) applies. ISO/TS 80004-1, Nanotechnologies - Vocabulary - Part 1: Core terms ISO/TS 80004-6, Nanotechnologies — Vocabulary — Part 6: Nano-object characterization ISO/TS 80004-13, Nanotechnologies — Vocabulary — Part 13: Graphene and other two-dimensional (2D) materials ISO 21363, Nanotechnologies — Measurements of particle size and shape distributions by transmission electron microscopy

3 Terms and definitions

For the purposes of this document, the terms and definitions given in ISO/TS 80004-1, ISO/TS 80004-6, ISO/TS 80004-13 and the following apply.

ISO and IEC maintain terminological databases for use in standardization at the following addresses:

  • ISO Online browsing platform: available at https:// www .iso .org/ obp
  • IEC Electropedia: available at https:// www .electropedia .org/

3.1 graphene

graphene layer single-layer graphene monolayer graphene 1LG single layer of carbon atoms with each atom bound to three neighbours in a honeycomb structure Note 1 to entry: Graphene is an important building block of many carbon nano-objects.

ISO/DTS 21356-2:2026(en) Note 2 to entry: As graphene is a single layer, it is also sometimes called monolayer graphene or single-layer graphene and abbreviated as 1LG to distinguish it from bilayer graphene (2LG) and few-layered graphene (FLG) Note 3 to entry: Graphene has edges and can have defects and grain boundaries where the bonding is disrupted. Note 4 to entry: In situations where the word graphene is used as an adjective, including in terms such as graphene enabled, the term commonly and incorrectly refers to GR2M and not just to single-layer graphene. [SOURCE: ISO/TS 80004-13:2024, 3.1.2.1]

3.2 graphite

allotropic form of the element carbon, consisting of graphene layers stacked parallel to each other in a threedimensional, crystalline, long-range order Note 1 to entry: Adapted from the definition in the IUPAC Compendium of Chemical Terminology. Note 2 to entry: There are two primary allotropic forms with different stacking arrangements: hexagonal and rhombohedral.

[SOURCE: ISO/TS 80004-13:2024, 3.1.2.2]

3.3 bilayer graphene

2LG two-dimensional material consisting of two well-defined stacked graphene layers Note 1 to entry: If the stacking registry is known, it can be specified separately, for example, as “Bernal stacked bilayer graphene”.

[SOURCE: ISO/TS 80004-13:2024, 3.1.2.7]

3.4 few-layer graphene

FLG two-dimensional material consisting of three to ten well-defined stacked graphene layers [SOURCE: ISO/TS 80004-13:2024, 3.1.2.11]

3.5 Bernal stacking

AB stacking hexagonal stacking <2D material> stacking of 2D material layers on top of one another in such a way that the neighbouring layers only have half of their atoms positioned equivalently in the out of plane direction with every third layer located in the same position in the out of plane axis Note 1 to entry: The second layer is horizontally displaced with respect to the first layer by half a lattice constant. [SOURCE: ISO/TS 80004-13:2024, 3.4.1.12]

3.6 stacking angle

<2D material> angle measured in the horizontal plane between the orientations of two layers of a 2D material that are stacked vertically on top of one another [SOURCE: ISO/TS 80004-13:2024, 3.4.1.14]

ISO/DTS 21356-2:2026(en)

3.7 turbostratic stacking

<2D material> stacking of layers of 2D materials that cannot be described as Bernal or rhombohedral stacking, instead having a relative stacking angle between the layers and which does not allow to develop atomic plane families other than that parallel to the basal plane, because the stacked layers exhibit a relative and random rotational angle or commensurate rotation between the layers Note 1 to entry: Correspondingly, the only diffraction peaks with three Miller indices seen in XRD patterns are 001 peaks (002, 004, etc.); the others are 2-indices only (typically 10 and 11). [SOURCE: ISO/TS 80004-13:2024, 3.4.1.15]

3.8 defect

<2D material> local deviation from regularity in the crystal lattice of a 2D material [SOURCE: ISO/TS 80004-13:2024, 3.4.1.1]

3.9 sheet

<2D material> 2D material typically situated upon a substrate, with extended lateral dimensions at the micro to macroscale [SOURCE: ISO/TS 80004-13:2024, 3.1.1.4]

3.10 Raman spectroscopy

spectroscopy in which the radiation scattered from a sample illuminated with monochromatic radiation is characterized by an energy loss or gain arising from rotational, or vibrational mode excitations [SOURCE: ISO 18115-3:2022, 3.5.17]

3.11 Raman shift

energy difference between inelastically scattered photon and incident photon resulting via Raman effect which is equal to the energy of the associated vibrational or rotational mode Note 1 to entry: Raman shift is typically expressed in wavenumbers [SOURCE: ISO 18115-3:2022, 3.5.19]

4 Abbreviated terms

For the purposes of this document, the following symbols and abbreviations apply. NOTE The final “M”, given as “Microscopy”, may be taken equally as “Microscope” depending on the context. 1D one-dimensional 1LG single layer graphene 2D two-dimensional 2LG bilayer graphene BF bright field CPD critical point drier CRM certified reference material

ISO/DTS 21356-2:2026(en) CVD chemical vapour deposition DI deionised FLG few-layer graphene FWHM full-width at half-maximum HRTEM high-resolution transmission electron microscopy NA numerical aperture PMMA polymethyl-methacrylate STEM scanning transmission electron microscopy SAED selected area electron diffraction TEM transmission electron microscopy

5 Sequence of measurement methods

This clause presents the sequence of measurement methods necessary to most efficiently characterize graphene sheets. Follow the sequence of events and measurement methods as outlined in Figure 1 to determine the structural properties of graphene sheets. The graphene sheet should be transferred to a silicon dioxide on silicon (Si/SiO ) substrate (Clause 6), if it is not already prepared as such, for optical

microscopy to be performed to measure surface coverage, as detailed in Clause 7. This is followed by Raman spectroscopy (see Clause 8), to determine coverage, number of layers and level of disorder. TEM should be undertaken after transfer of a different part of the same sheet, from the original copper or Si/ SiO substrate (Clause 6), onto an appropriate TEM grid. TEM, as detailed in Clause 9, will provide additional

information for a smaller area but will provide complementary information to the Raman spectroscopy measurements to more accurately understand the number of layers. TEM will also provide an understanding of the layer stacking, namely whether the material is Bernal stacked or turbostratic stacked. High-resolution TEM will also provide information on the type of defects present.

ISO/DTS 21356-2:2026(en) Figure 1 — Determining the structural properties of graphene sheets

6 Sample transfer and preparation

6.1 Introduction

The type of substrate that the graphene sheet is on shall be determined. If it matches the required substrate for analysis, then proceed to the relevant instrumentation clause. If not, a sample preparation process must be performed. Typically, CVD-grown graphene will be produced on a sacrificial copper substrate and must be removed from the copper before transfer using the procedure in Clause 6.2, which details a typical transfer procedure. This can be a copper wafer or a sheet used in a roll-to-roll production process, as just two examples. It should be noted that, typically, residue is left on the graphene sheet following these types of sample transfer processes.

For TEM imaging and SAED analysis, the required substrate is a TEM grid. For optical microscopy and Raman spectroscopy, the graphene sheet should be on a silicon dioxide on silicon substrate, with the oxide thickness of either 300 nm ± 5 nm or 90 nm ± 5 nm. This substrate must be cut to size and cleaned prior to use as detailed in Clause 6.4. If the graphene sample is provided on a Si/SiO substrate, it must be transferred to a

TEM grid before performing TEM measurements using the method detailed in Clause 6.3. Clause 6.5 details a sample and substrate preparation and transfer procedure for a sheet onto either a Si/ SiO substrate for optical microscopy and Raman spectroscopy or a holey carbon TEM support grid for TEM

analysis.

ISO/DTS 21356-2:2026(en)

6.2 Removal from copper substrate

In the case of CVD-grown graphene on copper, the graphene growth takes place on both sides of the metal substrate. It is therefore necessary to remove the graphene from one side, so that only one CVD-grown graphene sheet is transferred to another substrate. Use the following method:

a) The side being prepared for transfer should be covered with an approximately 300 nm layer of polymethyl-methacrylate (PMMA) using a spin coating system. This is in order to protect and support the underlying graphene during the transfer process. For example, the approximately 300 nm layer of PMMA can be produced at 3 000 rpm for 1 minute when using 950 000 molecular weight PMMA dissolved in Anisole (methyl phenyl ether) at 4 % dilution.

b) The other side of the sample should be exposed to approximately 2,7 Pa (20 mTorr) of oxygen plasma at 50 W for 3 minutes.

c) To minimize the contamination left on the graphene, a 0,1 mol L ammonium persulphate ((NH ) S O ) 4 2 2 8 solution should be used as an etchant to remove the copper foil, through a slow redox reaction over approximately 1 hour. The separation of the graphene film from the copper substrate is achieved through completely dissolving the copper, at which point the graphene layer attached to the PMMA film (PMMA/ graphene) will be floating at the surface of the solution, with the graphene layer on the underside of the PMMA.

d) After the etching procedure, the PMMA/graphene sample should be immersed in deionized (DI) water for 1 hour or more, followed by transfer to fresh DI water for further immersion for 1 hour or more, to remove any further contaminants and subsequent 1 hour DI water immersion steps can be undertaken where necessary.

6.3 Removal from silicon dioxide on silicon substrate

For TEM imaging, the graphene sheet can require being transferred from a Si/SiO substrate to a TEM grid.

If this is the case, use the following method:

a) The sheet being prepared for transfer should be covered with an approximately 300 nm layer of polymethyl-methacrylate (PMMA) using a spin coating system. This is in order to protect the underlying graphene and to ease the transfer process. As an example, an approximately 300 nm layer of PMMA can be produced at 3 000 rpm for 1 minute when using 950 000 molecular weight PMMA dissolved in Anisole at 4 % dilution.

b) The sample should then be baked in an oven at 130 °C for 5 minutes. c) The topmost layer of the Si/SiO substrate should then be etched away using a 3 % potassium hydroxide

(KOH) solution for approximately 6 hours at room temperature, so the PMMA/graphene film can be detached from the substrate in Step d).

d) Before the PMMA/graphene film has fully detached from the substrate, the Si/SiO wafer should be

immersed into a DI water bath, to fully detach the PMMA/graphene and to remove chemical residues from the etchant and possible contamination from the Si/SiO wafer. The PMMA/graphene film will

then float in the DI water.

e) The PMMA/graphene film should then be immersed in deionised (DI) water for 1 hour or more, followed by transfer to fresh DI water for further immersion for 1 hour or more. To ensure the best sample cleanliness possible, a further 1 hour DI water immersion steps can be undertaken where necessary.

6.4 Silicon wafer substrate preparation

a) Obtain a silicon wafer with a 90 nm or 300 nm oxide thickness. This thickness of oxide should be used due to its favourable optical conditions such that the transferred graphene sheet is more easily visible. b) Cut a section from the wafer to the size required, for example the same size as the graphene/PMMA sample. For example, this could be 1 cm × 1 cm and cut using a diamond scribe or wafer cutter.

ISO/DTS 21356-2:2026(en) c) Sonicate the substrate in acetone for 5 minutes, followed by a sonication step in deionised water for 5 minutes and finally in isopropyl alcohol for 5 minutes without drying the substrate between solvents. d) Dry the substrate using a pressurized source of nitrogen or argon gas. e) Inspect the substrate using optical microscopy to determine if any particles (≥ 500 nm) or solvent residue (observed as a different colour than the substrate) are present. If it is then repeat steps c) to e).

6.5 Sample and substrate preparation and transfer

After the PMMA/graphene sheet has been removed from the copper or Si/SiO substrate, it can then be

transferred onto either a Si/SiO substrate for optical microscopy and Raman spectroscopy (i.e. graphene

was removed from copper) or a holey carbon TEM support grid (i.e. graphene was removed from Si/SiO ),

for TEM analysis.

a) The PMMA/graphene layer should be removed from the deionised (DI) water bath by scooping it out with the desired substrate, held with tweezers.

b) A clean substrate should be used. This can be cleaned using plasma cleaning. 1) For TEM, use a TEM support grid consisting of holes in an amorphous carbon film supported on a metal (Cu or Au) mesh, typically with an overall diameter of 3 mm. TEM grids should be cleaned carefully prior to contact with graphene, by washing in isopropyl alcohol and vacuum baking the empty grids at approximately 120 °C for at least 30 minutes.

2) For Raman spectroscopy, use silicon dioxide on silicon wafer. This should be prepared prior to use using the method described in 6.4.

c) The graphene should be on the underside of the PMMA film unless the vertical orientation of the film has changed during the washing steps.

d) The substrate should be brought into contact with the graphene side of the PMMA/graphene layer. Care should be taken to prevent the graphene layer folding during transfer. 1) For TEM, the carbon side of the TEM support grid should be brought into contact with the graphene side of the PMMA/graphene to improve the likelihood of adhesion. 2) The field of view in the TEM is limited so it is important to ensure that the graphene region of interest is transferred within the central region of the support grid, typically >1 mm from the edge, as shown in Figure 2.

e) The sample should be dried at 50 °C for 10 minutes.

f) The sample should then be baked for 10 minutes at 120 °C in clean room conditions. This will improve the adhesion of the sheet on the substrate, remove the remaining water content, and importantly, flatten (anneal) possible wrinkles, which can be created during the transfer. g) The PMMA protective layer should then be dissolved by immersing the sample into acetone for 15 minutes. If there are any issues with cleanliness of the sample, an additional sample immersion step in ethanol for 15 minutes can be performed after the acetone immersion. h) After removing the PMMA, the sample should be supercritically dried, for example in a critical point drier (CPD). A CO medium should be used for the drying process due to its low critical temperature of

only 31 °C and low pressure 7,39 MPa, compared to 374 °C and 22,064 MPa for water. The CPD is used to protect the delicate, graphene sheet against any rupture, damage or deformation due to capillary forces during regular evaporative drying at ambient pressures. For the case of a TEM grid, a CPD prevents the volume change on evaporation from damaging the graphene membrane.

ISO/DTS 21356-2:2026(en) a) b) Key a low magnification b high magnification of the sample in Figure 2 a) NOTE Figure 2 b) shows both the support and holes in the mesh of the grid. Figure 2 — Optical microscopy images of CVD-grown graphene transferred onto a holey carbon TEM support grid

...

Contents

  • Introduction
  • 1 Scope
  • 2 Normative references
  • 3 Terms and definitions
  • 4 Abbreviated terms
  • 5 Sequence of measurement methods
  • 6 Sample transfer and preparation
  • 6.1 Introduction
  • 6.2 Removal from copper substrate
  • 6.3 Removal from silicon dioxide on silicon substrate
  • 6.4 Silicon wafer substrate preparation
  • 6.5 Sample and substrate preparation and transfer
  • 7 Determination of coverage of graphene using optical microscopy
  • 7.1 Introduction
  • 7.2 Measurement protocol
  • 7.3 Data analysis
  • 1 Graphene graphene
  • 2 Substratesubstrate
  • 8 Raman spectroscopy of a graphene sheet
  • 8.1 Introduction
  • 8.2 Instrumentation
  • 8.3 Measurement method
  • 8.4 Curve fitting
  • 8.5 Determination of graphene properties
  • 8.6 Reporting
  • 9 TEM and SAED of a graphene sheet
  • 9.1 Introduction
  • 9.2 Instrumentation
  • 9.3 Measurement protocol
  • 9.4 Data analysis
  • 1 TEM image from a contaminated sample
  • 2 SAED pattern from a contaminated sample
  • 3 TEM image from a torn sample
  • 4 SAED pattern from a torn sample
  • 5 TEM image from a creased sample
  • 6 SAED pattern from a creased sample
  • 7 TEM image from a sample with grain boundaries
  • 8 SAED pattern from a sample with grain boundaries
  • 10 Reporting
  • 10.1 General
  • 10.2 Sample preparation
  • 10.3 Raman spectroscopy
  • 10.4 TEM
  • Annex A
  • Annex B
  • Bibliography

Introduction

Graphene is starting to impact many different application areas such as solar cells, biosensors, displays, composites, flexible electronics and energy storage due to its exceptional properties. As industry uptake of this material increases, international standardization is critical to enable commercialization. Reliable, accurate, and reproducible measurements are important due to many production routes and producers of the material, in order to enable comparability and maintain high quality manufacture. There are, in general, two forms of commercially-available graphene, namely flakes/particles or a sheet on a substrate. The former are supplied in the form of a powder or liquid dispersion and can be flake-like in nature but can vary in lateral size and thickness, thus commercial-available material is also likely to contain thicker flakes classed as graphite. The structural characterization of these materials is described in ISO/TS 21356- 1:2021 ,Nanotechnologies — Structural characterization of graphene —Part 1: Graphene from powders and dispersions.

This document, the second part of the ISO/TS 21356 series, describes the structural characterization of graphene in the form of a sheet, predominantly produced via chemical vapour deposition (CVD), but applicable to graphene sheets produced using alternative methods, that can be transferred onto appropriate substrates. It provides a flow-chart for analysts to follow. It details the methods for characterizing the structural properties of graphene sheets in a systematic way. The methods used are optical microscopy, Raman spectroscopy and transmission electron microscopy (TEM). Note that graphene related two-dimensional materials deposited onto substates as particles from powders or liquid dispersions are not addressed in this document, but are addressed within ISO/TS 21356-1 “,Nanotechnologies — Structural characterization of graphene. Part 1: Graphene from powders and dispersions”..

The measurands determined are:

a) the percentage of substrate covered by graphene; b) the number of layers, ; c) the level of disorder; d) the layer stacking.

For each technique, sample preparation routines, measurement protocols and ways to analyze the data are provided.

ISO/DTS 21356-2:(en) Nanotechnologies — Structural characterization of graphene — — Part 2:

Graphene sheets on a substrate

1 Scope

This document details the methods for characterizing the structural properties of CVD-grown graphene, or graphene sheets produced using alternative methods, which can be transferred onto appropriate substrates. The methods used are optical microscopy, Raman spectroscopy, transmission electron microscopy (TEM) and selected area electron diffraction (SAED). The properties determined are the percentage of substrate covered by graphene, the number of layers, the level of disorder and the layer stacking. Sample preparation routines, measurement protocols and data analysis for the characterization of graphene sheets are provided.

2 Normative references

The following documents are referred to in the text in such a way that some or all of their content constitutes requirements of this document. For dated references, only the edition cited applies. For undated references, the latest edition of the referenced document (including any amendments) applies. ISO/TS 80004-1, Nanotechnologies - Vocabulary - Part 1: Core terms ISO/TS 80004-6, Nanotechnologies -— Vocabulary -— Part 6: Nano-object characterization ISO/TS 80004-13, Nanotechnologies -— Vocabulary -— Part 13: Graphene and other two-dimensional (2D) materials ISO 21363, Nanotechnologies — Measurements of particle size and shape distributions by transmission electron microscopy

3 Terms and definitions

For the purposes of this document, the terms and definitions given in ISO/TS 80004-1, ISO/TS 80004-6, ISO/TS 80004-13 and the following apply.

ISO and IEC maintain terminological databases for use in standardization at the following addresses:

  • — ISO Online browsing platform: available at https://www.iso.org/obp
  • — IEC Electropedia: available at https://www.electropedia.org/ 3.1 3.1 graphene graphene layer single-layer graphene monolayer graphene 1LG single layer of carbon atoms with each atom bound to three neighbours in a honeycomb structure Note 1 to entry: It Graphene is an important building block of many carbon nano-objects.

ISO/DTS 21356-2:(en) Note 2 to entry: As graphene is a single layer, it is also sometimes called monolayer graphene or single-layer graphene and abbreviated as 1LG to distinguish it from bilayer graphene (2LG) and few-layered graphene (FLG) Note 3 to entry: Graphene has edges and can have defects and grain boundaries where the bonding is disrupted. Note 4 to entry: In situations where the word graphene is used as an adjective, including in terms such as graphene enabled, the term commonly and incorrectly refers to GR2M and not just to single-layer graphene. [SOURCE: ISO/TS 80004-13:2024, 3.1.2.1] 3.2 3.2 graphite allotropic form of the element carbon, consisting of graphene layers stacked parallel to each other in a threedimensional, crystalline, long-range order Note 1 to entry: Adapted from the definition in the IUPAC Compendium of Chemical Terminology. Note 2 to entry: There are two primary allotropic forms with different stacking arrangements: hexagonal and rhombohedral.

[SOURCE: ISO/TS 80004-13:2024, 3.1.2.2] 3.3 3.3 bilayer graphene 2LG two-dimensional material consisting of two well-defined stacked graphene layers Note 1 to entry: If the stacking registry is known, it can be specified separately, for example, as “Bernal stacked bilayer graphene”.

[SOURCE: ISO/TS 80004-13:2024, 3.1.2.7] 3.4 3.4 few-layer graphene FLG two-dimensional material consisting of three to ten well-defined stacked graphene layers [SOURCE: ISO/TS 80004-13:202042024, 3.1.2.11] 3.5 3.5 Bernal stacking

AB stacking

hexagonal stacking

<2D material> stacking of 2D material layers on top of one another in such a way that the neighbouring layers only have half of their atoms positioned equivalently in the out of plane direction with every third layer located in the same position in the out of plane axis Note 1 to entry: The second layer is horizontally displaced with respect to the first layer by half a lattice constant. [SOURCE: ISO/TS 80004-13:2024(en),, 3.4.1.12]

ISO/DTS 21356-2:(en) 3.6 3.6

stacking angle

<2D material> angle measured in the horizontal plane between the orientations of two layers of a 2D material that are stacked vertically on top of one another [SOURCE: ISO/TS 80004-13:2024(en),, 3.4.1.14] 3.7 3.7

turbostratic stacking

<2D material> stacking of layers of 2D materials that cannot be described as Bernal or rhombohedral stacking, instead having a relative stacking angle between the layers and which does not allow to develop atomic plane families other than that parallel to the basal plane, because the stacked layers exhibit a relative and random rotational angle or commensurate rotation between the layers Note 1 to entry: Correspondingly, the only diffraction peaks with three Miller indices seen in XRD patterns are 001 peaks (002, 004, etc.); the others are 2-indices only (typically 10 and 11). [SOURCE: ISO/TS 80004-13:2024(en),, 3.4.1.15] 3.8 3.8

defect

<2D material> local deviation from regularity in the crystal lattice of a 2D material. [SOURCE: ISO/TS 80004-13:2024(en),, 3.4.1.1] 3.9 3.9

sheet

<2D material> 2D material typically situated upon a substrate, with extended lateral dimensions at the micro to macroscale [SOURCE: ISO/TS 80004-13:2024(en),, 3.1.1.4] 3.10 3.10

Raman spectroscopy

spectroscopy in which the radiation scattered from a sample illuminated with monochromatic radiation is characterized by an energy loss or gain arising from rotational, or vibrational mode excitations [SOURCE: ISO 18115-3:2022(en),, 3.5.17] 3.11 3.11

Raman shift

energy difference between inelastically scattered photon and incident photon resulting via Raman effect which is equal to the energy of the associated vibrational or rotational mode

ISO/DTS 21356-2:(en) Note 1 to entry: Raman shift is typically expressed in wavenumbers [SOURCE: ISO 18115-3:2022(en),, 3.5.19]

4 Abbreviated terms

For the purposes of this document, the following symbols and abbreviations apply. NOTE The final “M”, given as “Microscopy”, may be taken equally as “Microscope” depending on the context. 1D one-dimensional 1LG single layer graphene 2D two-dimensional 2LG bilayer graphene BF bright field CPD critical point drier CRM certified reference material CVD chemical vapour deposition DI deionised FLG few-layer graphene FWHM full-width at half-maximum HRTEM high-resolution transmission electron microscopy NA numerical aperture PMMA polymethyl-methacrylate STEM scanning transmission electron microscopy SAED selected area electron diffraction TEM transmission electron microscopy 1D one-dimensional 1LG single layer graphene 2D two-dimensional 2LG bilayer graphene BF bright field CPD critical point drier CRM certified reference material CVD chemical vapour deposition DI deionised FLG few-layer graphene FWHM full-width at half-maximum HRTEM high-resolution transmission electron microscopy NA numerical aperture

ISO/DTS 21356-2:(en) PMMA polymethyl-methacrylate STEM scanning transmission electron microscopy SAED selected area electron diffraction TEM transmission electron microscopy

5 Sequence of measurement methods

This clause presents the sequence of measurement methods necessary to most efficiently characterize graphene sheets. Follow the sequence of events and measurement methods as outlined in Figure 1Figure 1 to determine the structural properties of graphene sheets. The graphene sheet should be transferred to a silicon dioxide on silicon (Si/SiO ) substrate (Clause 6(Clause 6),), if it is not already prepared as such, for optical

microscopy to be performed to measure surface coverage, as detailed in Clause 7Clause 7.. This is followed by Raman spectroscopy (see Clause 8Clause 8),), to determine coverage, number of layers and level of disorder. TEM should be undertaken after transfer of a different part of the same sheet, from the original copper or Si/SiO substrate (Clause 6(Clause 6),), onto an appropriate TEM grid. TEM, as detailed in Clause 9Clause 9,,

will provide additional information for a smaller area but will provide complementary information to the Raman spectroscopy measurements to more accurately understand the number of layers. TEM will also provide an understanding of the layer stacking, namely whether the material is Bernal stacked or turbostratic stacked. High-resolution TEM will also provide information on the type of defects present.

ISO/DTS 21356-2:(en)

ISO/DTS 21356-2:(en)

Figure 1 — — Determining the structural properties of graphene sheets

6 Sample transfer and preparation

6.1 Introduction

The type of substrate that the graphene sheet is on shall be determined. If it matches the required substrate for analysis, then proceed to the relevant instrumentation clause. If not, a sample preparation process will need tomust be performed. Typically, CVD-grown graphene will be produced on a sacrificial copper substrate and will need tomust be removed from the copper before transfer using the procedure in Clause 6.2Clause 6.2,, which details a typical transfer procedure. This can be a copper wafer or a sheet used in a roll-to-roll production process, as just two examples. It should be noted that, typically, residue is left on the graphene sheet following these types of sample transfer processes.

For TEM imaging and SAED analysis, the required substrate is a TEM grid. For optical microscopy and Raman spectroscopy, the graphene sheet should be on a silicon dioxide on silicon substrate, with the oxide thickness of either 300 nm ± ± 5 nm or 90 nm ± ± 5 nm. This substrate will need tomust be cut to size and cleaned prior to use as detailed in Clause 6.4Clause 6.4.. If the graphene sample is provided on a Si/SiO2 substrate, it will need tomust be transferred to a TEM grid before performing TEM measurements using the method detailed in Clause 6.3Clause 6.3..

Clause 6.5Clause 6.5 details a sample and substrate preparation and transfer procedure for a sheet onto either a Si/SiO2 substrate for optical microscopy and Raman spectroscopy or a holey carbon TEM support grid for TEM analysis.

ISO/DTS 21356-2:(en)

6.2 Removal from copper substrate

In the case of CVD-grown graphene on copper, the graphene growth takes place on both sides of the metal substrate. It is therefore necessary to remove the graphene from one side, so that only one CVD-grown graphene sheet is transferred to another substrate. Use the following method:

a) The side being prepared for transfer should be covered with a ~an approximately 300 nm layer of polymethyl-methacrylate (PMMA) using a spin coating system. This is in order to protect and support the underlying graphene during the transfer process. For example, the ~approximately 300 nm layer of PMMA can be produced at 3 000 rpm for 1 minute when using 950 000 molecular weight PMMA dissolved in Anisole (methyl phenyl ether) at 4 % dilution.

b) The other side of the sample should be exposed to ~approximately 2,7 Pa (20 mTorr) of oxygen plasma at 50 W for 3 minutes.

c) To minimize the contamination left on the graphene, a 0,1 mol L ammonium persulphate ((NH ) S O ) 4 2 2 8 solution should be used as an etchant to remove the copper foil, through a slow redox reaction over ~approximately 1 hour. The separation of the graphene film from the copper substrate is achieved through completely dissolving the copper, at which point the graphene layer attached to the PMMA film (PMMA/graphene) will be floating at the surface of the solution, with the graphene layer on the underside of the PMMA.

d) After the etching procedure, the PMMA/graphene sample should be immersed in deionized (DI) water for 1 hour or more, followed by transfer to fresh DI water for further immersion for 1 hour or more, to remove any further contaminants and subsequent 1 hour DI water immersion steps can be undertaken where necessary.

6.3 Removal from silicon dioxide on silicon substrate

For TEM imaging, the graphene sheet may have to becan require being transferred from a Si/SiO2 substrate to a TEM grid. If this is the case, use the following method:

a) The sheet being prepared for transfer should be covered with a ~an approximately 300 nm layer of polymethyl-methacrylate (PMMA) using a spin coating system. This is in order to protect the underlying graphene and to ease the transfer process. As an example, a ~an approximately 300 nm layer of PMMA can be produced at 3 000 rpm for 1 minute when using 950 000 molecular weight PMMA dissolved in Anisole at 4 % dilution.

b) The sample should then be baked in an oven at 130 °C for 5 minutes. c) The topmost layer of the Si/SiO2 substrate should then be etched away using a 3 % potassium hydroxide (KOH) solution for approximately 6 hours at room temperature, so the PMMA/graphene film can be detached from the substrate in Step d).

d) Before the PMMA/graphene film has fully detached from the substrate, the Si/SiO2 wafer should be immersed into a DI water bath, to fully detach the PMMA/graphene and to remove chemical residues from the etchant and possible contamination from the Si/SiO wafer. The PMMA/graphene film will then float

in the DI water.

e) The PMMA/graphene film should then be immersed in deionised (DI) water for 1 hour or more, followed by transfer to fresh DI water for further immersion for 1 hour or more. To ensure the best sample cleanliness possible, a further 1 hour DI water immersion steps can be undertaken where necessary.

ISO/DTS 21356-2:(en)

6.4 Silicon wafer substrate preparation

a) Obtain a silicon wafer with a 90 nm or 300 nm oxide thickness. This thickness of oxide should be used due to its favourable optical conditions such that the transferred graphene sheet is more easily visible. b) Cut a section from the wafer to the size required, for example the same size as the graphene/PMMA sample. For example, this could be 1 cm × 1 cm and cut using a diamond scribe or wafer cutter. c) Sonicate the substrate in acetone for 5 minutes, followed by a sonication step in deionised water for 5 minutes and finally in isopropyl alcohol for 5 minutes without drying the substrate between solvents. d) Dry the substrate using a pressurized source of nitrogen or argon gas. e) Inspect the substrate using optical microscopy to determine if any particles (≥ 500 nm) or solvent residue (observed as a different colour than the substrate) are present. If it is then repeat steps c) to e).

6.5 Sample and substrate preparation and transfer

After the PMMA/graphene sheet has been removed from the copper or Si/SiO substrate, it can then be

transferred onto either a Si/SiO substrate for optical microscopy and Raman spectroscopy (i.e. graphene was

removed from copper) or a holey carbon TEM support grid (i.e. graphene was removed from Si/SiO ), for TEM

analysis.

a) The PMMA/graphene layer should be removed from the deionised (DI) water bath by scooping it out with the desired substrate, held with tweezers.

b) A clean substrate should be used. This can be cleaned using plasma cleaning. 1) For TEM, use a TEM support grid consisting of holes in an amorphous carbon film supported on a metal (Cu or Au) mesh, typically with an overall diameter of 3 mm. TEM grids should be cleaned carefully prior to contact with graphene, by washing in isopropyl alcohol and vacuum baking the empty grids at ~approximately 120 °C for at least 30 minutes.

2) For Raman spectroscopy, use silicon dioxide on silicon wafer. This should be prepared prior to use using the method described in 6.46.4. .

c) The graphene should be on the underside of the PMMA film unless the vertical orientation of the film has changed during the washing steps.

d) The substrate should be brought into contact with the graphene side of the PMMA/graphene layer. Care should be taken to prevent the graphene layer folding during transfer. 1) For TEM, the carbon side of the TEM support grid should be brought into contact with the graphene side of the PMMA/graphene to improve the likelihood of adhesion. 2) The field of view in the TEM is limited so it is important to ensure that the graphene region of interest is transferred within the central region of the support grid, typically >1 mm from the edge, as shown in Figure 2Figure 2. .

e) The sample should be dried at 50 °C for 10 minutes.

f) The sample should then be baked for 10 minutes at 120 °C in clean room conditions. This will improve the adhesion of the sheet on the substrate, remove the remaining water content, and importantly, flatten (anneal) possible wrinkles, which could have beencan be created during the transfer.

ISO/DTS 21356-2:(en) g) The PMMA protective layer should then be dissolved by immersing the sample into acetone for 15 minutes. If there are any issues with cleanliness of the sample, an additional sample immersion step in ethanol for 15 minutes can be performed after the acetone immersion. h) After removing the PMMA, the sample should be supercritically dried, for example in a critical point drier (CPD). A CO medium should be used for the drying process due to its low critical temperature of only

31 °C and low pressure 7,39 MPa, compared to 374 °C and 22,064 MPa for water. The CPD is used to protect the delicate, graphene sheet against any rupture, damage or deformation due to capillary forces during regular evaporative drying at ambient pressures. For the case of a TEM grid, a CPD prevents the volume change on evaporation from damaging the graphene membrane.

a) b) Key

...