Abstract

This document specifies a test method to determine the resistance to wear of lacquered wood floorings, a method to test the elasticity of the lacquer and a method to determine resistance to impact of lacquered wood floorings.

Status
Not Published
Publication Date
28-Jun-2027
Current Stage
4060 - Closure of enquiry - Enquiry
Start Date
01-Oct-2026
Due Date
11-Jun-2026
Completion Date
11-Jun-2026

Buy Documents

Draft

prEN 13696:2026 - BARVE

English language (50 pages)
Preview
Preview
e-Library read for
×1 day

prEN 13696 is a draft European Standard from CEN for test methods on wood flooring with lacquered surfaces. It covers wear resistance, lacquer elasticity, impact resistance, and resistance to scratching/scraping so that the surface performance of flooring products can be compared in a repeatable way. Laboratories, manufacturers, and flooring suppliers use it for product development, batch checks, and test reports.

What does prEN 13696 specify?

prEN 13696 specifies test methods for lacquered wood floorings and for wooden flooring surfaces with filmforming coatings. The document gives common conditioning and lacquer-thickness measurement methods, then sets out specific methods for wear, elasticity, scratching/scraping, and impact resistance.

The structure is straightforward:

  • Clauses 1 to 3 cover scope, normative references, and terms.
  • Clause 4 gives common methods.
  • Clauses 5 and 6 give two different wear-resistance methods.
  • Clause 7 covers elasticity of the lacquer.
  • Clause 8 covers resistance to scratching and scraping.
  • Clause 9 covers impact resistance.
  • Annex A is informative and adds a sand paper CS 17 wear-resistance method.
AnnexWhat it covers
ASand paper CS 17 wear resistance method, with its own sampling, apparatus, calibration, procedure, result expression, and test report content

What are the key requirements of prEN 13696?

Common preparation and lacquer thickness

Clause 4.1 sets the conditioning climate at 23 °C and 50 % relative humidity, with tolerances given in the document. The manufacturer specifies which of the listed conditioning climates applies, and the test equipment and materials are stabilised in the same atmosphere. In practice, this reduces variation caused by moisture and temperature.

Clause 4.2 measures lacquer thickness with an optical instrument and a marked edge on the test piece. The thickness check is used as context for wear and elasticity results, so the lab can report not only how a surface behaves but also how much lacquer was present.

Wear resistance by falling sand and by sand paper

Clause 5 uses a falling sand method with loaded wheels and loose abrasive grit. It is mainly intended for lacquers without antiabrasive materials such as corundum. The method requires calibration of grit flow and abrasive capacity, so the number of rotations to wear-through is based on a controlled abrasive action rather than on machine drift.

Clause 6 uses abrasive paper strips with rubber-covered wheels and is mainly intended for lacquers with antiabrasive materials such as corundum. The abrasive paper batch is checked on a zinc calibration plate before testing. The result is the initial wear point, reported from the number of revolutions, so the test shows when a harder lacquered surface first opens up.

Both wear methods use three test specimens taken from one floor covering element when possible. The sampling pattern and the position of the joint, when one is needed, matter because the test is meant to reflect the finished product, not just a convenient cut piece.

Elasticity of the lacquer

Clause 7 uses a steel indentation plate with 12 cones of different heights. The test piece or full-size element is loaded until the cones are in full contact, then the lacquer is inspected for cracking. The key result is the highest cone height that causes a crack, which gives a practical measure of how well the lacquer follows deformation without breaking.

Clause 7 also links elasticity with lacquer thickness. Four surrounding pieces are used for thickness measurement, and ten areas or test pieces are used for batch elasticity results. For a reader, this means the method is not just about whether cracking occurs, but also about whether the coating thickness is consistent enough to support the result.

Scratch and scrape resistance

Clause 8 applies to non-structured wooden flooring surfaces with filmforming coatings, and it can also be used for other flooring surfaces with filmforming coatings. The scratch-plane tester uses an indexable insert at a 55° cutting angle, and the force is increased stepwise until damage appears, then reduced to find the highest force with no visible damage.

The assessment is done under diffuse light at a specified illumination level, and the operator looks for scratches and scrapes of at least 10 mm. Grooves, dents, and gloss changes without scratches or scrapes are not counted as relevant damage. That distinction matters because the result is intended to reflect visible surface damage, not every mark made during the test.

Impact resistance

Clause 9 tests the ability of the surface layer to withstand a dropped object. A polished stainless steel ball of a stated mass and diameter is dropped from different heights onto five specimens, and the result is the average maximum height that produces no damage. The underlay used in the test follows the manufacturer’s installation intent or the supplied underlay, which makes the result closer to real use.

What terms does prEN 13696 define?

  • Lacquer - a film-forming agent that modifies the surface layer properties and has a measurable thickness.
  • Film forming coating - the coating term used for coated wooden flooring surfaces in clause 8.
  • Scratch - line-shaped damage where the substrate is exposed after the scratch-plane tester passes over the coating.
  • Groove - deformation of the substrate and coating without a scratch or scrape being formed.
  • Relevant damage - scratches and scrapes with a minimum length of 10 mm.
  • Non relevant damage - grooves, dents, or gloss changes that occur without scratches or scrapes.

Who uses prEN 13696?

prEN 13696 is used by testing laboratories, flooring manufacturers, coating developers, and quality managers who need comparable data on lacquered wood flooring surfaces. Buyers, specifiers, and certification teams use the results when they want to compare products, verify a batch, or check a declared performance level. The methods are also relevant to suppliers that need to document how a lacquer behaves under wear, scratching, and impact.

What changed in prEN 13696 from the previous edition?

prEN 13696 supersedes EN 13696:2008. The foreword states two changes: integration of new abrasion methods and an editorial update of the document.

Which standards are used with prEN 13696?

  • EN 13756:2018 - provides wood flooring and parquet terminology used in clause 3, including the coating terminology used in clause 8.
  • EN ISO 291:2018 - provides the standard atmospheres for conditioning and testing used in clauses 4, 8, and 9.
  • EN ISO 868:2003 - provides the hardness method used for the leather abrading wheels in the falling sand wear method.
  • EN ISO 6506-1 - provides the Brinell hardness test used for the zinc calibration plate in the sand paper method and Annex A.
  • ISO 48-6 and ISO 48-7 - provide hardness methods used for the rubber-covered abrasive wheels in the sand paper wear method.
  • EN ISO 3668 - supports the visual assessment conditions in the scratch and scrape test.
  • ISO 24338:2022, Annex A and EN 13329:2016+A2:2021, Annex F and G - are cited for calibration, maintenance, and hardness measurement details for Taber-style abrader equipment.
  • EN ISO 7784-2:2023 and ASTM D785 - support the CS 17 wear method in Annex A, including abrasive wheels, regeneration, and calibration plate hardness.
  • CEN ISO/TR 21555:2020 - is the source for the scratch definition used in clause 8.

What does the prEN 13696 document contain?

prEN 13696 contains detailed apparatus descriptions, sampling layouts, conditioning instructions, and result-expressions for each test method. It includes figures for the specimen layouts, abrasion machines, templates, indentation plate, scratch-plane tester, and impact apparatus, so a laboratory can set up the test equipment in a consistent way.

The document also contains calibration and maintenance steps for abrasive systems, including grit flow checks, abrasive capacity checks, and wheel checks. That matters because the same flooring can give different wear results if the abrasive system is out of control.

Tables in the document support the technical details, including cone heights for the elasticity plate and material or grain specifications for abrasive media. Annex A adds its own procedure and report items for the CS 17 wear-resistance method.

Relations

Effective Date
26-Jun-2024

Buy Documents

Draft

prEN 13696:2026 - BARVE

English language (50 pages)
Preview
Preview
e-Library read for
×1 day

Get Certified

Connect with accredited certification bodies for this standard

Gozdarski inštitut Slovenije

Slovenian Forestry Institute. Forest management certification support, timber testing.

SA Slovenia Verified

Sponsored listings

Frequently Asked Questions

prEN 13696 is a draft published by the European Committee for Standardization (CEN). Its full title is "Wood flooring - Test methods to determine elasticity and resistance to wear and impact resistance and scratching/scraping". This standard covers: This document specifies a test method to determine the resistance to wear of lacquered wood floorings, a method to test the elasticity of the lacquer and a method to determine resistance to impact of lacquered wood floorings.

This document specifies a test method to determine the resistance to wear of lacquered wood floorings, a method to test the elasticity of the lacquer and a method to determine resistance to impact of lacquered wood floorings.

prEN 13696 is classified under the following ICS (International Classification for Standards) categories: 79.080 - Semi-manufactures of timber; 97.150 - Floor coverings. The ICS classification helps identify the subject area and facilitates finding related standards.

prEN 13696 has the following relationships with other standards: It is inter standard links to EN 13696:2008. Understanding these relationships helps ensure you are using the most current and applicable version of the standard.

prEN 13696 is available in PDF format for immediate download after purchase. The document can be added to your cart and obtained through the secure checkout process. Digital delivery ensures instant access to the complete standard document.

Standards Content (Sample)

Contents

  • 1 Scope
  • 2 Normative references
  • 3 Terms and definitions
  • 3.1 lacquer
  • 4 Common methods
  • 4.1 Conditioning
  • 4.2 Measurement of the thickness of the lacquer
  • 5 Falling sand wear resistance method
  • 5.1 Principle
  • 5.2 Sampling
  • 5.3 Conditioning
  • 5.4 Apparatus testing machine
  • 5.5 Grit feeder and accessories
  • 5.6 Procedure
  • 5.7 Test report
  • 6 Sand paper wear resistance method
  • 6.1 Principal
  • 6.2 Sampling
  • 6.3 Conditioning
  • 6.4 Apparatus
  • 6.5 Procedure
  • 7 Elasticity of the lacquer
  • 7.1 Principle
  • 7.2 Equipment
  • 7.3 Test piece
  • 7.4 Procedure
  • 7.5 Expression of the results for a test piece
  • 7.6 Expression of the result for a batch
  • 7.7 Test report
  • 8 Determination of resistance to scratching and scraping
  • 8.1 Principle
  • 8.2 Terms and definitions
  • 8.3 Equipment
  • 8.4 Preparation of apparatus
  • 8.5 Preparation of test pieces
  • 8.6 Test procedure
  • 8.7 Assessment
  • 8.8 Test report
  • 9 Impact resistance
  • 9.1 Principle
  • 9.2 Apparatus
  • 9.3 Test specimens
  • 9.4 Conditioning
  • 9.5 Procedure
  • 9.6 Expression of results
  • 9.7 Test report
  • Annex A
  • Bibliography

1 Scope

This document specifies a test method to determine the resistance to wear of lacquered wood floorings, a method to test the elasticity of the lacquer and a method to determine resistance to impact of lacquered wood floorings.

2 Normative references

The following documents are referred to in the text in such a way that some or all of their content constitutes requirements of this document. For dated references, only the edition cited applies. For undated references, the latest edition of the referenced document (including any amendments) applies. EN 13756:2018, Wood flooring and parquet — Terminology EN ISO 291:2018, Plastics — Standard atmospheres for conditioning and testing (ISO 291:2008) EN ISO 868:2003, Plastics and ebonite — Determination of indentation hardness by means of a durometer (Shore hardness) (ISO 868:2003) EN ISO 6506-1, Metallic materials — Brinell hardness test — Part 1: Test method (ISO 6506-1) ISO 48-6, Rubber, vulcanized or thermoplastic — Determination of hardness — Part 6: Apparent hardness of rubber-covered rollers by IRHD method ISO 48-7, Rubber, vulcanized or thermoplastic — Determination of hardness — Part 7: Apparent hardness of rubber-covered rollers by Shore-type durometer method

3 Terms and definitions

For the purposes of this document, the following terms and definitions given in EN 13756 and the following apply.

ISO and IEC maintain terminology databases for use in standardization at the following addresses:

  • ISO Online browsing platform: available at https://www.iso.org/obp/
  • IEC Electropedia: available at https://www.electropedia.org/

3.1 lacquer

film making agent modifying surface layer properties Note 1 to entry: It has a measurable thickness.

4 Common methods

4.1 Conditioning

4.1.1 Equipment

Enclosures with the following climatic conditions:

  • climate temperature of (23 ± 2) °C and relative humidity of (50 ± 5) %.

oSIST prEN 13696:2026 prEN 13696:2026 (E)

4.1.2 Procedure

The manufacturer shall specify either of the conditioning climates above. Unless otherwise specified, all equipment and materials required for the test shall be stabilised and kept in an enclosure in the climate specified.

4.2 Measurement of the thickness of the lacquer

4.2.1 Equipment
4.2.1.1 Optical instrument

An instrument with a resolution of at least ±2 μm.

NOTE For instance, a binocular microscope with a magnification of 100 to 200 and a built-in measuring scale in the field of view.

4.2.1.2 Contrast marking

A water-based felt tip pen.

4.2.2 Sampling

Choose the location from which the test pieces are taken, depending on the purpose of the measurement (either in an unworn area or in a worn area).

Test pieces with a size at least 10 mm × 10 mm and by the full thickness shall be cut out of one of the wear test pieces or area to be tested in elasticity.

The number of test pieces is specified in 5.3.3.4.1 and 6.4.1.

4.2.3 Procedure

If needed, contrast mark the lacquered face with the felt-tip pen specified in 4.2.1.2. Clear-cut with a razor blade the edge of the lacquered face to be inspected. Mount the test piece with the clear-cut edge facing the microscope. For each test piece, make at least two measurements to the accuracy allowed by the resolution of the optical instrument. Measurements of lacquer above open holes in the wood shall not be taken into account.

4.2.4 Expression of the results

When required, average the measurements made on each test piece. If there is more than one test piece, calculate to one significant figure the mean value and the coefficient of variation (expressed as a percentage) of the results.

5 Falling sand wear resistance method

5.1 Principle

The resistance to wear is evaluated by abrading the face of representative lacquered test pieces or lacquered specimens with a specified abrasive sand applied by means of two loaded wheels. The number of rotations, necessary to reach a defined wear, is used to evaluate the resistance to wear. NOTE This test is mainly used for lacquers without antiabrasive materials like corundum.

oSIST prEN 13696:2026 prEN 13696:2026 (E)

5.2 Sampling

One floor covering element is needed. Take from this element three test pieces, measuring approximately 100 mm × 100 mm:

  • two centred 10 mm in from the short edges; and
  • one exactly in the centre of the element (see Figure 1).

Machined edges and machined surfaces shall be avoided in the pieces. If the thickness of the test pieces exceeds 8 mm the specimens shall be milled down from the backside to (7,5 ± 0,5) mm to ensure a horizontal load of the abrader arms. Make sure that specimens are uniformly flat and parallel after milling.

If the dimension of the elements makes the described sampling impossible, the test pieces shall be sampled from the nearest available area. If the elements measure less than 100 mm, then a joint is necessary. The joint shall be positioned in the middle of the 100 mm × 100 mm pieces.

Figure 1 — Sampling from one floor covering element Drill a (7,2 ± 0,1) mm centre hole into the test pieces.

5.3 Conditioning

The test pieces shall be conditioned to constant mass in one of the climates defined in 4.1. Prior to testing, the lacquer shall be fully cured according to the manufacturer's instructions.

5.4 Apparatus testing machine

5.4.1 General

The testing machine shall consist of the items specified in 5.4.2 to 5.4.4.

5.4.2 Test piece holder

In form of a disc with a diameter of approximately 105 mm (item 4 in Figure 3) which rotates in a horizontal plane with a permitted deviation of ±2 mm/m at a frequency of 58/min to 62/min and to which the test specimen (item 3 in Figure 3) can be clamped with a clamping screw (item 11 in Figure 3).

5.4.3 Holding and lifting device

Holding and lifting device (item 7 in Figure 3) for the abrasive wheels, so constructed that each wheel exerts a force of (10 ± 0,2) N on the test specimen.

oSIST prEN 13696:2026 prEN 13696:2026 (E) A counterweight of (150 ± 3) g is required to counterbalance the mass of the leather abrading wheel (5.4.3). A second pair of leather abrading wheels may be used for this purpose. The calibration and maintenance of the Taber abrader arms should be carried out according to ISO 24338:2022, Annex A.

5.4.4 Revolution-counter

A revolution counter is needed to record the number of revolutions of the specimen holder.

5.5 Grit feeder and accessories

5.5.1 General

A Grit feeder shall have a minimum storage capacity of about 200 g of grit. It shall be possible to open it at the top and at the bottom. The bottom opening shall be positioned (10 ± 1) mm above the face of the test piece and have a length of (16 ± 1) mm and width of (3,18 ± 0,38) mm. The length of the bottom opening shall be installed radially to the test specimen holder. To make sure of a regular flow, a device shall be provided in the grit feeder to ensure a regular flow. A further device ensuring an immediate stop of the feeding is also required (see Figure 2 and Figure 3).

5.5.2 Vacuum cleaning device

A suction nozzle positioned (3 ± 2) mm above the track to be worn, shall be installed in the axial vertical plane behind the left wheel after the abrasive grit passes under the wheel (relative to the rotation direction; see Figure 3). The vacuum power shall remove all dust and debris but shall not influence the flow of falling grit.

NOTE Equipment of this type, Taber Abrader and Taber Grit Feeder, are made by TABER Industries, 455 Bryant

Street, North Tonawanda, New York 14120 USA.

1) This information is given for the convenience of users of this document and does not constitute an endorsement by CEN of this product. Equivalent products may be used if they can be shown to lead to the same results.

oSIST prEN 13696:2026 prEN 13696:2026 (E)

Figure 2 — Example of a Taber abrader with grit feeder

oSIST prEN 13696:2026 prEN 13696:2026 (E) Dimensions in millimetres

Key 1 grit nozzle 7 abrader arm 2 suction nozzle 8 counterweight 3 test piece 9 wearing surface 4 specimen holder 10 direction of rotation 5 testing weight 11 clamping screw 6 abrading wheel 12 nut Figure 3 — Abrader with grit feeder

oSIST prEN 13696:2026 prEN 13696:2026 (E)

5.5.3 Abrading material

Electric arc furnaced Aluminium Oxide, bauxite based abrasive grain with a chemical composition

according to Table 1. The abrasive mineral has a specific gravity of 3,96 g/cm and a hardness of

21 kN/mm (Knoop). The medium grain shape of the mineral has a bulk density according to FEPA

standard 44-1 in the range of 1,51 - 1,62 g/cm . Particle size distribution ranges between 45 µm and 75 µm with a reduced fines portion according to Table 2 determined according to FEPA standard 42-1. Table 1 — Chemical composition Chemicals Al2O3 Fe2O3 SiO2 TiO2 CaO ZrO2 MgO Chemical proportion % > 95 < 0,30 < 0,90 2,4 to 3,0 < 0,30 < 0,30 < 0,30 Table 2 — Grain distribution Sieve No. 170 200 270 270 - 325 325 Grading µm 90 75 53 45 Grain distribution % 0 0 to 5 ≥ 45 ≥ 80 0 to 10

NOTE The abrading material “ALODUR ESK 240 (EN 14354)”, made by Treibacher Schleifmittel, Postfach 1, A- 2) 9523 Villach-Landskron Seebach 2, Austria, is an example of a suitable product available commercially. The abrading material shall be used only once. Do not sieve the abrading material before use. The abrading material shall be stored in a dry place.

5.5.4 Leather abrading wheels

Two cylindrical wheels free to turn on their axis with nominal diameter and width of respectively 44,4 mm and 12,7 mm. They are fitted with a leather strip having a width of (12,7 ± 0,1) mm and a minimum thickness of 1,5 mm. The overall diameter of the wheels, with leather strips shall not exceed 50,8 mm or be less than 47,4 mm.

The hardness of the leather strips shall be suitable for the purpose. It is measured according to the procedure in EN ISO 868 with a Shore-Durometer of Type A with the following deviations:

  • the Shore-A hardness is measured at four points in the middle of the tire tread of abrading wheels (instead of the requirements in EN ISO 868:2003, 5.1, 5.2 and 8.1).
  • the hardness of the leather is suitable if all the results are contained within the range A/1:85 – A/1:95.

The distance between the internal faces of the wheels shall be (52,5 ± 0,2) mm, their common axis being set, by (19,05 ± 0,3) mm nominally, off the axis of the specimen holder. The axis of rotation of the test piece shall be equidistant from the two wheels.

Prior to testing, new abrading wheels shall be preconditioned. Subject new wheels to an initial 2 000 cycle test following the procedure described in 6.5.4.

2) This information is given for the convenience of users of this document and does not constitute an endorsement by CEN of this product. Equivalent products may be used if they can be shown to lead to the same results.

oSIST prEN 13696:2026 prEN 13696:2026 (E) NOTE The abrading wheels “S-39”, made by TABER Industries are an example of a suitable product available

commercially.

5.5.5 Stopwatch

A stopwatch accurate to ±0,1 s.

5.5.6 Grit collection container

A container of known mass to collect the grit when calibrating the grit feeder.

5.5.7 Calibration plates

Calibration plates made of cell-cast acrylics with Rockwell Hardness M 94 according to ASTM D785. NOTE The calibration plates “S38”, made by TABER Industries, are an example of a suitable product available 4) commercially.

5.5.8 Transparent template to evaluate the wear of the abraded area

Transparent template for visual observation of wear through. Each quadrant is divided into four sectors of 22,5° (see Figure 4).

Figure 4 — Transparent template for visual observation of wear through

5.5.9 Weighing equipment

For determining the mass loss of the calibration plate by the sand or calibrating the grit flow of the abrading material, weighing equipment with an accuracy of ±1 mg is needed.

3) This information is given for the convenience of users of this document and does not constitute an endorsement by CEN of this product. Equivalent products may be used if they can be shown to lead to the same results. 4) This information is given for the convenience of users of this document and does not constitute an endorsement by CEN of this product. Equivalent products may be used if they can be shown to lead to the same results.

oSIST prEN 13696:2026 prEN 13696:2026 (E)

5.5.10 Contrast marking solutions

Water solution of methyl blue 0,1 % by mass fraction.

5.6 Procedure

5.6.1 General

A specified loose abrasive is fed continuously on to the face of the test piece, in the track of the loaded wheels. As the specimen rotates the rub / wear action of the wheels and abrasive grit causes abrasion on the test piece. After passing under both wheels, the loose abrasive is removed by a vacuum.

5.6.2 Maintenance of the abrading wheels

The abrading wheels may be used as long as the specifications described in 5.4.4 are complied with. When they are not, the wheels shall be removed and replacement shall be carried out.

5.6.3 Operation of the abrader

To start the wear test:

  • fix the test piece on the specimen holder;
  • position the vacuum cleaning nozzle, start the vacuum;
  • position the bottom opening of the grit feeder;
  • set the revolution counter (5.4.4) to zero;
  • lower the abrading wheels to the surface of the test piece;
  • open the grit feeder, with the rate of grit flow calibrated as specified in 5.4.4;
  • start rotation of the test piece;
  • check if the sandfall is radial to the abrasion area.

To halt the wear test:

  • stop rotation of the test piece;
  • close the grit feeder;
  • stop the vacuum;
  • raise the abrading wheels;
  • record the number of revolutions.
5.6.4 Calibration
5.6.4.1 Rate of grit flow

Before each test, calibrate the grit flow from the grit feeder by means of:

  • the container specified in 5.5.6;

oSIST prEN 13696:2026 prEN 13696:2026 (E) - a stopwatch as specified in 5.5.5; - weighing equipment as specified in 5.5.9.

The grit flow shall last for (60 ± 1) s.

Collect and weigh the quantity of grit that flowed from the grit feeder. Be certain to subtract the mass of the container from this measurement.

The grit feeder is properly calibrated if the measured mass is (21 ± 3) g. This calibration shall be repeated after each test piece or 5 000 revolutions or each break that lasts longer than 30 min.

5.6.4.2 Abrading capacity

For every new package of abrading material, the abrading capacity shall be checked. Start a wear test in accordance with the procedure defined in 5.4.3, the test piece being replaced by the calibration plate specified in 5.5.7.

Wipe clean the calibration plate with a soft cloth that has been dampened with an antistatic spray. Measure the initial mass of the calibration plate, and then secure the calibration plate to the specimen holder.

Operate the abrader for 2 000 revolutions. Replenish the abrading material as necessary. Determine the difference between the initial mass of the calibration plate and the mass after 2 000 revolutions. Repeat the test two additional times with an untested side of a calibration plate (each side of the plate may be used only one time).

Calculate the average of the three mass loss measurements.

The result is acceptable if:

  • the average loss of mass is (145 ± 40) mg;
  • no individual measurement is beyond the range (145 ± 50) mg. After 25 000 revolutions, the abrading capacity shall be repeated and the result shall be checked. After each checking of the abrading capacity calculate the calibration factor as follows:

Calibration factor = average of mass loss in g / 0,145 g.

Test equipment and materials.

5.6.4.3 Test procedure

5.6.4.3.1 Initial thickness of the lacquer Measure it in accordance with the method specified in 4.2.

The initial thickness is required only for information. Use one test piece only. 5.6.4.3.2 Wear through Prior to the wear test, condition the test piece as specified in 4.1.2. The wear test is carried out in the same climate.

Run the abrader as specified in 5.5.3. until the occurrence of the wear through of the lacquer. Evaluate wear through by placing the transparent template (see 5.5.8) on the test piece and examining visually. If the contrast between the substrate and the lacquer is not sufficient, use the contrast making

oSIST prEN 13696:2026 prEN 13696:2026 (E) solution specified in 5.5.10. The liquid should be spread on the surface, and removed with a dry paper in order to colour the surface abraded and distinguish it from not completely abraded surface Wear through has occurred when the support shows:

  • through 12 sectors out of 16; and
  • through 1 sector per quadrant.

Inspect the test piece after every 200 revolutions. When the test nears its end, inspect after every 100 revolutions.

Compare the examined test surface with the examples for wear trough points and deviations described in Figure 5, examples for abrasion.

(1) Insufficient test (2) Correct test (3) Excessive test Wear through is not reached Wear in 12 of 16 sectors and Wear-through has passed (no abrasion in 12 sectors) in every quadrant beyond 12 sectors Figure 5 — Assessment of Wear trough At specimens with a joint, wear through within 10 mm of the centre joint shall be disregarded.

5.6.5 Expression of the result for a test piece
5.6.5.1 Initial thickness of the lacquer

See 4.2.4.

5.6.5.2 Single wear through value

For each specimen tested, multiply the number of total revolutions with the calibration factor determined in 5.4.2 to obtain corrected single test values. Expression of the result for a batch.

5.6.5.3 Initial thickness of the lacquer

See 4.2.4.

5.6.5.4 Average wear through value

The result is average of the individual numbers of rotations to wear the lacquer through each test piece (see 5.3) rounded to the previous hundred.

oSIST prEN 13696:2026 prEN 13696:2026 (E)

5.7 Test report

It shall contain the following information:

  • name and address of laboratory;
  • name and address of company ordering the test;
  • reference to this document, i.e. EN 13696;
  • sampling procedure and identification of the sample;
  • date of delivery;
  • relevant dates of test(s);
  • type of lacquer and its nominal thickness;
  • material tested (wood species, lay-up, manufacturer);
  • nominal dimensions for tested material;
  • conditioning and test climate;
  • single and average wear trough values;
  • other conditions that may be of significance in interpreting the results, e.g. noticeable change in appearance.

6 Sand paper wear resistance method

6.1 Principal

This paragraph specifies a test method to determine the wear resistance of lacquered surfaces using the sand paper method.

NOTE This test is mainly used for lacquers with antiabrasive materials like corundum.

6.2 Sampling

One floor covering element is needed. Take from this element three test specimens, measuring approximately 100 mm × 100 mm:

  • two centred 10 mm in from the short edges; and
  • one exactly in the centre of the element (see Figure 6).

Machined edges and machined surfaces shall be avoided in the specimens. If the thickness of the specimens exceeds 8 mm the specimens shall be milled down from the backside to (7,5 ± 0,5) mm to ensure a horizontal load of the abrader arms. Make sure that specimens are uniformly flat and parallel after milling.

If the dimension of the elements makes the described sampling impossible, the test specimens shall be sampled from the nearest available area. If the elements measure less than 100 mm, then a joint is necessary. The joint shall be positioned in the middle of the 100 mm × 100 mm specimen.

oSIST prEN 13696:2026 prEN 13696:2026 (E) Drill a (7,2 ± 0,1) mm centre hole into the test specimen.

Dimensions in millimetres

...