SIST EN ISO 14577-1:2026
(Main)Metallic materials - Instrumented indentation test for hardness and materials parameters - Part 1: Test method (ISO 14577-1:2026)
- Abstract
This document specifies the method of instrumented indentation test for determination of hardness and other materials parameters for the following three ranges:
macro range: 2 N ≤ F ≤ 30 kN;
micro range: 2 N > F; h > 0,2 µm;
nano range: h ≤ 0,2 µm.
For the nano range, the mechanical deformation strongly depends on the real shape of indenter tip and the calculated material parameters are significantly influenced by the contact area function of the indenter used in the testing machine. Therefore, careful calibration of both instrument and indenter shape is required in order to achieve an acceptable reproducibility of the materials parameters determined with different machines.
The macro and micro ranges are distinguished by the test forces in relation to the indentation depth.
Attention is drawn to the fact that the micro range has an upper limit given by the test force (2 N) and a lower limit given by the indentation depth of 0,2 µm.
The determination of hardness and other material parameters is given in the normative Annex A.
At high contact pressures, damage to the indenter is possible. For test pieces with very high hardness and modulus of elasticity, permanent indenter deformation can occur and can be detected using suitable reference materials. Indentations that result in damage or permanent deformation of the indenter are excluded from the scope of this test method.
This test method can also be applied to thin metallic and non-metallic coatings and non-metallic materials. In this case, it is recommended that the specifications in the relevant standards be taken into account (see also 7.3 and ISO 14577-4).
The analysis methods of this standard assume that materials behave like ideal materials. Any deviation (internal stress, pile-up, sink-in, densification, phase transitions, cracks) will result in additional uncertainties. This becomes especially important if comparisons shall be done to material parameters, obtained with other methods.
- Status
- Published
- Public Enquiry End Date
- 29-Sep-2024
- Publication Date
- 16-Sep-2026
- Technical Committee
- PKG - Testing of metallic materials
- Current Stage
- 6060 - National Implementation/Publication (Adopted Project)
- Start Date
- 03-Jul-2026
- Due Date
- 07-Sep-2026
- Completion Date
- 17-Sep-2026
SIST EN ISO 14577-1:2026 is a European Standard published by CEN that specifies the test method for instrumented indentation on metallic materials. It covers how to determine hardness and other materials parameters from force and indentation-depth data, for use in the macro, micro, and nano ranges. For nanoindentation especially, the standard makes clear that indenter shape and calibration strongly affect results, so it is aimed at laboratories and users who need comparable indentation data.
What does SIST EN ISO 14577-1:2026 specify?
SIST EN ISO 14577-1:2026 specifies the method for instrumented indentation testing of metallic materials and explains how the document is organized. The main body runs from Scope through Test report, and the annexes provide the calculation methods, calibration topics, uncertainty guidance, and supporting notes.
| Annex | What it covers |
|---|---|
| Annex A | Materials parameters derived from force/indentation-depth data |
| Annex B | Types of control used for the indentation process |
| Annex C | Machine compliance and indenter area function |
| Annex D | Notes on diamond indenters |
| Annex E | Influence of surface roughness on result accuracy |
| Annex F | Correlation of indentation hardness H to Vickers hardness |
| Annex G | Determination of drift and minimizing creep influence |
| Annex H | Estimation of uncertainty of calculated hardness and materials parameters |
| Annex I | Calculation of radial displacement correction |
The scope includes macro range, micro range, and nano range testing. It also notes that the method can be applied to thin metallic and non-metallic coatings and to non-metallic materials when relevant standards are taken into account, especially for coating work.
What are the key requirements of SIST EN ISO 14577-1:2026?
Indentation ranges, indenter choice, and what the test measures
SIST EN ISO 14577-1:2026 separates testing into three ranges: macro, micro, and nano. The nano range is the most sensitive to the real tip shape and the area function of the indenter, so results depend heavily on calibration of both the instrument and the indenter.
The standard allows several indenter shapes for hardness testing, including Vickers, modified Berkovich, ball, and spherical tipped conical indenters. The indenter has to be harder than the test piece and must not suffer permanent deformation or damage during testing. That matters in practice because damaged indenters can distort the contact area and make results non-comparable.
Testing machine and calibration
SIST EN ISO 14577-1:2026 requires a machine that can apply the chosen force or displacement, measure force, indentation depth, and time throughout the cycle, and compensate for machine compliance. The machine must also use the appropriate indenter area function and meet the requirements of ISO 14577-2.
For users, this means the machine setup is not just about applying load - it must be able to record the full indentation history and correct for frame deformation. That is especially important when comparing different machines or using shallow indentations.
Test piece preparation and geometry
SIST EN ISO 14577-1:2026 requires a suitable test surface that is free from contamination and prepared so that surface changes from polishing or heating are minimized. Surface roughness matters more as indentation depth gets smaller, and Annex E links acceptable roughness to indentation depth.
The test surface should be normal to the indenter axis within 1°. The test piece also has to be thick enough, or the indentation shallow enough, to avoid support effects; for hardness and modulus measurements, the thickness must be at least 10 times the indentation depth or 3 times the indentation diameter, whichever is greater. In practice, this is the key rule that prevents the backing material or thin substrate from biasing the result.
Test cycle, zero point, drift, and spacing
SIST EN ISO 14577-1:2026 lets the test be force-controlled or displacement-controlled, including constant strain rate loading. The complete cycle has to be documented, including hold periods, loading rates, and logging frequency. The zero point, meaning first contact between indenter and surface, must be assigned for each test and its uncertainty reported.
Temperature and drift control are also central. Tests are to be carried out within stable temperature conditions, and if thermal drift would change the maximum indentation depth by more than 1 % during the cycle, the displacement data must be corrected. The standard also requires enough spacing between indentations and from edges or interfaces so previous impressions do not influence the measurement.
Uncertainty and reporting
SIST EN ISO 14577-1:2026 requires uncertainty evaluation in accordance with ISO/IEC Guide 98-3. The uncertainty budget should consider zero-point assignment, force and displacement noise, curve fitting, thermal drift, surface roughness, calibration, machine compliance, indenter area function, temperature effects, and surface tilt.
The test report has to identify the test piece, indenter, test cycle, result, expanded uncertainty, analysis methods, and any deviations or events that could have affected the result. In practice, this is what makes the data usable for quality records, comparisons between labs, and audits.
What terms does SIST EN ISO 14577-1:2026 use?
- Indentation hardness, H - hardness calculated from the maximum force and the projected contact area under load.
- Martens hardness, HM - hardness determined from the force/indentation-depth curve during loading, including elastic and plastic deformation.
- Indentation modulus, E - a modulus derived from unloading data that reflects the contact response of the test piece.
- Indentation creep, C - the relative change in indentation depth while force is held constant.
- Indentation relaxation, R - the relative change in force while indentation depth is held constant.
- Contact depth, h_c - the derived depth used to calculate contact area under load.
- Projected area of contact under load, A_p,c(h) - the contact area used in the hardness and modulus calculations.
- Machine compliance - elastic deformation of the testing machine that adds to the measured indentation depth and must be corrected.
Who uses SIST EN ISO 14577-1:2026?
SIST EN ISO 14577-1:2026 is used by materials testing laboratories, mechanical testing technicians, quality control and quality assurance teams, and engineering groups that need hardness, modulus, creep, or relaxation data from indentation tests. It is also relevant to buyers and manufacturers of metals, coatings, and test equipment who need results that can be compared across instruments and sites.
In practice, users apply it to method setup, machine verification, calibration checks, surface preparation, testing thin coatings, and reporting results with uncertainty. It is especially useful when optical measurement of the indent is not practical and the full load-depth-time curve is needed instead.
What changed in SIST EN ISO 14577-1:2026 from the previous edition?
SIST EN ISO 14577-1:2026 supersedes EN ISO 14577-1:2015. The foreword states these main changes:
- better specification of tip approach speed
- addition of a loading method with constant strain rate
- hardness definitions reordered, with H before HM
- improved guidance for tip cleaning
- clearer distinction between contact area under load and in the unloaded state
- complete reformulation of normative Annex I on radial displacement correction
Which standards are used with SIST EN ISO 14577-1:2026?
- ISO 14577-2:2026 - gives the verification and calibration rules for testing machines, including compliance and area function checks.
- ISO/IEC Guide 98-3:2008 - provides the framework for expressing measurement uncertainty used in Clause 9 and Annex H.
- ISO 14577-4 - is pointed to for test work on coatings, especially thin metallic and non-metallic coatings.
- ISO 14577-3 - is listed as the part covering calibration of reference blocks.
What does the SIST EN ISO 14577-1:2026 document contain?
SIST EN ISO 14577-1:2026 contains the test principle, machine requirements, specimen requirements, procedure, uncertainty rules, and the reporting items that have to be recorded. It also includes the symbols table and schematic figures for the indentation cycle, control modes, drift, and radial displacement effects.
A major part of the document is Annex A, which shows how to derive H, HM, E, creep, relaxation, and indentation work from the force/indentation-depth record. Annex C and Annex I are particularly important for practical work because they address machine compliance, indenter area function, and radial displacement correction. Annex E and Annex G deal with surface roughness and drift, which are common sources of error in real testing.
Relations
- Effective Date
- 01-Oct-2026
- Effective Date
- 01-Jul-2026
- Effective Date
- 01-Jul-2026
Get Certified
Connect with accredited certification bodies for this standard

Element Materials Technology
Materials testing and product certification.

Inštitut za kovinske materiale in tehnologije
Institute of Metals and Technology. Materials testing, metallurgical analysis, NDT.
Sponsored listings
Frequently Asked Questions
SIST EN ISO 14577-1:2026 is a standard published by the Slovenian Institute for Standardization (SIST). Its full title is "Metallic materials - Instrumented indentation test for hardness and materials parameters - Part 1: Test method (ISO 14577-1:2026)". This standard covers: This document specifies the method of instrumented indentation test for determination of hardness and other materials parameters for the following three ranges: macro range: 2 N ≤ F ≤ 30 kN; micro range: 2 N > F; h > 0,2 µm; nano range: h ≤ 0,2 µm. For the nano range, the mechanical deformation strongly depends on the real shape of indenter tip and the calculated material parameters are significantly influenced by the contact area function of the indenter used in the testing machine. Therefore, careful calibration of both instrument and indenter shape is required in order to achieve an acceptable reproducibility of the materials parameters determined with different machines. The macro and micro ranges are distinguished by the test forces in relation to the indentation depth. Attention is drawn to the fact that the micro range has an upper limit given by the test force (2 N) and a lower limit given by the indentation depth of 0,2 µm. The determination of hardness and other material parameters is given in the normative Annex A. At high contact pressures, damage to the indenter is possible. For test pieces with very high hardness and modulus of elasticity, permanent indenter deformation can occur and can be detected using suitable reference materials. Indentations that result in damage or permanent deformation of the indenter are excluded from the scope of this test method. This test method can also be applied to thin metallic and non-metallic coatings and non-metallic materials. In this case, it is recommended that the specifications in the relevant standards be taken into account (see also 7.3 and ISO 14577-4). The analysis methods of this standard assume that materials behave like ideal materials. Any deviation (internal stress, pile-up, sink-in, densification, phase transitions, cracks) will result in additional uncertainties. This becomes especially important if comparisons shall be done to material parameters, obtained with other methods.
This document specifies the method of instrumented indentation test for determination of hardness and other materials parameters for the following three ranges: macro range: 2 N ≤ F ≤ 30 kN; micro range: 2 N > F; h > 0,2 µm; nano range: h ≤ 0,2 µm. For the nano range, the mechanical deformation strongly depends on the real shape of indenter tip and the calculated material parameters are significantly influenced by the contact area function of the indenter used in the testing machine. Therefore, careful calibration of both instrument and indenter shape is required in order to achieve an acceptable reproducibility of the materials parameters determined with different machines. The macro and micro ranges are distinguished by the test forces in relation to the indentation depth. Attention is drawn to the fact that the micro range has an upper limit given by the test force (2 N) and a lower limit given by the indentation depth of 0,2 µm. The determination of hardness and other material parameters is given in the normative Annex A. At high contact pressures, damage to the indenter is possible. For test pieces with very high hardness and modulus of elasticity, permanent indenter deformation can occur and can be detected using suitable reference materials. Indentations that result in damage or permanent deformation of the indenter are excluded from the scope of this test method. This test method can also be applied to thin metallic and non-metallic coatings and non-metallic materials. In this case, it is recommended that the specifications in the relevant standards be taken into account (see also 7.3 and ISO 14577-4). The analysis methods of this standard assume that materials behave like ideal materials. Any deviation (internal stress, pile-up, sink-in, densification, phase transitions, cracks) will result in additional uncertainties. This becomes especially important if comparisons shall be done to material parameters, obtained with other methods.
SIST EN ISO 14577-1:2026 is classified under the following ICS (International Classification for Standards) categories: 77.040.10 - Mechanical testing of metals. The ICS classification helps identify the subject area and facilitates finding related standards.
SIST EN ISO 14577-1:2026 has the following relationships with other standards: It is inter standard links to SIST EN ISO 14577-1:2015, SIST EN 62788-1-6:2017/A1:2020, SIST EN ISO 14577-4:2008. Understanding these relationships helps ensure you are using the most current and applicable version of the standard.
SIST EN ISO 14577-1:2026 is available in PDF format for immediate download after purchase. The document can be added to your cart and obtained through the secure checkout process. Digital delivery ensures instant access to the complete standard document.
Standards Content (Sample)
Contents
- Introduction
- 1 Scope
- 2 Normative references
- 3 Terms and definitions
- 4 Symbols and designations
- 5 Principle
- 6 Testing machine
- 7 Test piece
- 8 Procedure
- 9 Uncertainty of the results
- 10 Test report
- Annex A
- Annex B
- Annex C
- Annex D
- Annex E
- Annex F
- Annex G
- 2 E dt
- Annex H
- Annex I
- 2 E E E
- Bibliography
Introduction
Hardness has typically been defined as the resistance of a material to permanent penetration by another harder material. The results obtained when performing Rockwell, Vickers, and Brinell tests are determined after the test force has been removed. Therefore, the effect of elastic deformation under the indenter has been ignored.
ISO 14577 (all parts) has been prepared to enable the user to evaluate the indentation of materials by considering both the force and displacement during plastic and elastic deformation. By monitoring the complete cycle of increasing and removal of the test force, hardness values equivalent to traditional hardness values can be determined. More significantly, additional properties of the material, such as its indentation modulus and elasto-plastic hardness, can also be determined. All these values can be calculated without the need to measure the indent optically. Furthermore, by a variety of techniques, the instrumented indentation test allows to record hardness and modulus depth profiles within a, probably complex, indentation cycle. Although the indentation modulus (E ) value obtained in this test method is not directly equivalent to IT Young’s modulus or the orientation specific elastic modulus of the material indented, E is, however, IT equivalent to the isotropic Hill average of the elastic plane strain modulus of the material when there is no pile up and no residual stress.
ISO 14577 (all parts) has been written to allow a wide variety of post-test data analysis. Part 1 of ISO 14577 specifies the method of indentation test for determination of instrumented indentation hardness and material properties.
SIST EN ISO 14577-1:2026
SIST EN ISO 14577-1:2026 International Standard ISO 14577-1:2026(en) Metallic materials — Instrumented indentation test for hardness and materials parameters — Part 1:
Test method
1 Scope
This document specifies the method of instrumented indentation test for determination of hardness and other materials parameters for the following three ranges:
- macro range: 2 N ≤ F ≤ 30 kN;
- micro range: 2 N > F; h > 0,2 µm;
- nano range: h ≤ 0,2 µm.
For the nano range, the mechanical deformation strongly depends on the real shape of indenter tip and the calculated material parameters are significantly influenced by the contact area function of the indenter used in the testing machine. Therefore, careful calibration of both instrument and indenter shape is required in order to achieve an acceptable reproducibility of the materials parameters determined with different machines.
The macro and micro ranges are distinguished by the test forces in relation to the indentation depth. Attention is drawn to the fact that the micro range has an upper limit given by the test force (2 N) and a lower limit given by the indentation depth of 0,2 µm.
The determination of hardness and other material parameters is given in the normative Annex A. At high contact pressures, damage to the indenter is possible. For test pieces with very high hardness and modulus of elasticity, permanent indenter deformation can occur and can be detected using suitable reference materials. Indentations that result in damage or permanent deformation of the indenter are excluded from the scope of this test method.
This test method can also be applied to thin metallic and non-metallic coatings and non-metallic materials. In this case, it is recommended that the specifications in the relevant standards be taken into account (see also 7.3 and ISO 14577-4).
The analysis methods of this standard assume that materials behave like ideal materials. Any deviation (internal stress, pile-up, sink-in, densification, phase transitions, cracks) will result in additional uncertainties. This becomes especially important if comparisons shall be done to material parameters, obtained with other methods.
2 Normative references
The following documents, in whole or in part, are normatively referenced in this document and are indispensable for its application. For dated references, only the edition cited applies. For undated references, the latest edition of the referenced document (including any amendments) applies. ISO 14577-2:2026, Metallic materials — Instrumented indentation test for hardness and materials parameters - Part 2: Verification and calibration of testing machines
SIST EN ISO 14577-1:2026 ISO 14577-1:2026(en) ISO/IEC Guide 98-3:2008, Uncertainty of measurement — Part 3: Guide to the expression of uncertainty in me a s ur ement (GUM: 1995)
3 Terms and definitions
No terms and definitions are listed in this document.
ISO and IEC maintain terminology databases for use in standardization at the following addresses:
- ISO Online browsing platform: available at https:// www .iso .org/ obp
- IEC Electropedia: available at https:// www .electropedia .org/
4 Symbols and designations
For the purposes of this document, the symbols and designations in Table 1 shall be applied (see also Figure 1 and Figure 2).
Table 1 — Symbols and designations Symbol Designation Unit
A (h ) Projected area of contact under load of the indenter at distance h from the tip mm p c c
Projected area of contact in unloaded state of the indenter at distance h from the mm
A (h ) p,UL c tip
A (h) Surface area of the indenter at distance h from the tip in unloaded state mm s C Indentation creep % IT Total measured compliance of the contact (dh/dF tangent to the force removal nm/mN C T curve at maximum test force) C Machine compliance nm/mN F C Compliance of the contact after correction for machine compliance nm/mN S E Indentation modulus of the test piece GPa IT Reduced plane strain modulus of the contact (combination of test piece and in- GPa E r denter plane strain moduli) F Test force N F Maximum test force N max h Indentation depth under applied test force mm h Contact depth of the indenter with the test piece at F mm c max h Maximum indentation depth at F mm max max h Permanent indentation depth after removal of the test force mm p Point of intersection of the tangent c to curve b at F with the indentation mm max h r depth-axis as identified on Figure 1 H Indentation hardness GPa IT HM Martens hardness GPa Martens hardness, determined from the slope of the increasing GPa HM s force/indentation depth curve GPa HM Martens hardness, determined from the first derivative of h vs F diff ν Poisson’s ratio of the test piece s r Radius of spherical indenter mm R Indentation relaxation % IT NOTE 1 To avoid very long numbers, the use of multiples or sub-multiples of the units can be used. 2 2 NOTE 2 The continued use of the unit N/mm is allowed. 1 MPa = 1 N/mm .
SIST EN ISO 14577-1:2026 ISO 14577-1:2026(en) TTabablele 1 1 ((ccoonnttiinnueuedd)) Symbol Designation Unit W Elastic reverse deformation work of indentation N⋅m elast W Total mechanical work of indentation N⋅m total Cone semi-angle or angle of facet to the indentation axis for pyramidal ° α indenters Maximum angle between the contact surface and the indenter for calculation of ° θ radial displacement η Ratio W /W % IT elast total NOTE 1 To avoid very long numbers, the use of multiples or sub-multiples of the units can be used. 2 2 NOTE 2 The continued use of the unit N/mm is allowed. 1 MPa = 1 N/mm .
a Application of the test force.
b Removal of the test force.
Tangent to curve b at F .
max Figure 1 — Schematic representation of the test procedure
SIST EN ISO 14577-1:2026 ISO 14577-1:2026(en) Key a Indenter.
b Surface of residual plastic indentation in a test piece that has a “perfectly plastic” response.
Surface of test piece at maximum indentation depth and test force. θ maximum angle between the test piece surface and the indenter Figure 2 — Schematic representation of the cross section of indentation in the case of material “sink-in”
5 Principle
Continuous recording of the force and the depth of indentation permits the determination of hardness and material properties (see Figure 1 and Figure 2). The measured values of hardness and other material parameters shall be determined in accordance with Annex A. An indenter consisting of a material harder than the material under test shall be used (i.e. the indenter shall not permanently deform and shall not be damaged as a result of indentation). For hardness testing the following shapes and materials can be used:
a) indenter shaped as an orthogonal pyramid with a square base and with an angle α = 68° between the axis of the diamond pyramid and one of the faces (Vickers pyramid; see Figure A.1); b) pyramid with triangular base (e.g. modified Berkovich pyramid with an angle α = 65,27° between the axis of the diamond pyramid and one of the faces; see Figure A.1); c) ball indenter (especially for the determination of the elastic behaviour of materials); d) spherical tipped conical indenter.
This document does not preclude the use of other indenter geometries; however, care should be taken when interpreting the results obtained with such indenters. Diamond is the preferred material but other materials like sapphire may also be used for example to avoid chemical reaction between the indenter and the test piece, provided the above mechanical requirements of the indenter are met. For indentation modulus testing, the indenter geometries for hardness testing are strongly recommended but, in principle, any geometry indenter may be used provided that the area function is known and the area function is monotonically increasing with indentation depth.
NOTE Due to the crystal structure of diamond, indenters that are intended to be spherical are often polyhedrons and do not have an ideal spherical shape.
The test procedure can either be force-controlled or displacement-controlled. The test force, F, the corresponding indentation depth, h, and time are recorded during the whole test procedure. The result of the test is the data set of the test force and the relevant indentation depths as a function of time (see Figure 1 and Annex B).
For a reproducible determination of the force and corresponding indentation depth, the zero point for the force/indentation depth measurement shall be assigned individually for each test (see 7.3).
SIST EN ISO 14577-1:2026 ISO 14577-1:2026(en) Where time-dependent effects are being measured - using the force-controlled method, the test force is kept constant over a specified period and the change of the indentation depth is measured as a function of the holding time of the test force (see Figures A.3 and B.1), and - using the indentation depth-controlled method, the indentation depth is kept constant over a specified period and the change of the test force is measured as a function of the holding time of the indentation depth (see Figures A.4 and B.2).
The two kinds of control mentioned give essentially different results in the segment b of the curves in Figure B.1 a) and Figure B.2 b) or in Figure B.1 b) and Figure B.2 a).
6 Testing machine
6.1 The testing machine shall have the capability of applying predetermined test forces or displacements within the required scope and shall fulfil the requirements of ISO 14577-2. 6.2 The testing machine shall have the capability of measuring and reporting applied force, indentation displacement and time throughout the testing cycle.
6.3 The testing machine shall have the capability of compensating for the machine compliance and of utilizing the appropriate indenter area function according to Annex C and ISO 14577-2:2026, 5.5 and 5.6. 6.4 Indenters for use with testing machines can have various shapes, as specified in ISO 14577-2 (for further information on indenters, see Annex D).
6.5 The testing machine shall operate at a temperature within the permissible range specified in 7.1 and shall maintain its calibration within the limits specified in ISO 14577-2:2026, Clause 5.
7 Test piece
7.1 The test shall be carried out on a region of the test surface that allows the determination of the force/ indentation depth curve for the respective indentation range within the required uncertainty. The contact area shall be free of fluids or lubricants except where this is essential for the performance of the test, in which case, this shall be described in detail in the test report. Care shall be taken that extraneous matter (e.g. dust particles) is not incorporated into the contact.
Generally, provided the surface is free from obvious surface contamination, cleaning procedures should be avoided. If cleaning is required, it shall be limited to the following methods to minimize damage:
- application of a dry, oil-free, filtered gas stream;
- application of a subliming particle stream of CO (but keeping the surface temperature above the dew
point); - rinsing with a solvent (which is chemically inert to the test piece) and then setting it to dry. If these methods fail and the surface is sufficiently robust, wipe the surface with a lint-free tissue soaked in solvent to remove trapped dust particles, after which, the surface shall be rinsed in a solvent as above. Ultrasonic methods are known to create or increase damage to surfaces and coatings and should only be used with caution.
Surface finish has a significant influence on the test results that depends upon the relative size of the indentation depth, h, with respect to the arithmetic mean deviation roughness, Ra. The relative size of these parameters shall conform to the limits given in Annex E.
SIST EN ISO 14577-1:2026 ISO 14577-1:2026(en) The test piece surface shall be normal to the test force direction. The angle difference between test surface normal and indenter axis shall be less than 1°. The effect of surface tilt should be included in the uncertainty calculation.
The sample should be free from magnetism. Test pieces capable of becoming magnetised should be checked for magnetism and demagnetised before testing, if possible. Precautions should be taken to avoid the effect of magnetism on the measuring system.
7.2 If necessary, preparation of the test surface shall be carried out in such a way that any alteration of the surface hardness and/or surface residual stress (e.g. due to heat or cold-working) is minimized. Due to the small indentation depths in the micro and nano range, special precautions shall be taken during the test piece preparation. When polishing is needed, a polishing process that is suitable for the particular materials shall be used.
Electropolishing is a recommended preparation method that can remove a work hardened surface layer. However, care should be taken that the surface roughness does not exceed the limits given in this standard. 7.3 The test piece thickness shall be large enough (or indentation depth small enough) such that the test result is not influenced by the test piece support. For hardness and modulus measurements, the test piece thickness shall be at least 10 times the indentation depth or 3 times the indentation diameter (see 8.7), whichever is greater. For modulus measurements a sample thickness larger than 30 times the indentation depth is recommended. For measurements of thinner samples, it is recommended to follow the analysis described in ISO 14577-4 for coatings.
When testing coatings, the coating thickness should be considered as the test piece thickness. For testing thin samples or coatings, see ISO 14577-4 for better testing procedures. NOTE The above are empirically based limits based on hardness testing. The effect of test piece thickness on the elastic modulus result is not the same as the effect on the hardness result. The exact limits of influence of support on test piece depend on the geometry of the indenter used and the materials properties of the test piece and support.
8 Procedure
8.1 The temperature of the test shall be recorded. Tests shall be performed within ±10 °C of the temperature of the instrument calibration.
The temperature stability during a test is more important than the actual test temperature. Any calibration correction applied shall be reported along with the additional calibration uncertainty. It is recommended that tests, particularly in the nano and micro ranges, be performed in controlled conditions, in the range (23 ± 5) °C and (45 ± 10) % relative humidity.
The individual tests, however, shall be carried out at stable temperature conditions because of the requirement of high depth measuring accuracy. This means that:
- the test pieces shall have reached the ambient temperature before testing,
- the testing machine shall have reached a stable working temperature (operating manual should be consulted),
- the ambient, instrument, and test temperature shall be within the range for which the machine calibration is valid, and
- other external influences causing temperature changes during individual test have been controlled. To minimize thermally induced displacement drift, the temperature of the testing machine shall be adequately maintained over the time period of one testing cycle, or a displacement drift shall be measured and corrected. A decision tree to assist in estimating the drift during the experiment is shown in Figure 3. If the drift rate is significant, the displacement data shall be corrected by measuring the drift rate during a hold at an applied force as close to zero force as is practicable or during a hold at a suitable place in the
SIST EN ISO 14577-1:2026 ISO 14577-1:2026(en) force removal curve in accordance with Annex G and ISO 14577-2:2026, 5.3.3). In all cases where the drift rate would influence the maximum indentation depth by more than 1 % within the total indentation cycle time, the drift rate shall be corrected (see tolerances in ISO 14577-2:2026, Table 2 and 5.3.3). If a contact in the fully elastic regime can be obtained, a hold at initial contact is preferred. In this way, material influences (creep, visco-plasticity, cracking) can be minimized. When the measurement is significantly longer than the hold period for thermal drift measurement it is recommended to measure the thermal drift before and after the experiment and to correct the displacement using the average of the two drift rates. The difference between the two drift rates is an estimate of the drift rate uncertainty. The uncertainty due to the drift, or in the drift correction used, shall be reported.
To determine the drift of surface referenced instruments, contact between the reference indenter and the sample surface shall be elastic. This may be determined by calculation. NOTE The significance of a particular drift rate upon the measurement depends upon the range of the indentation and the type of application.
Figure 3 — Decision tree to assist in estimating thermal drift using a constant force hold period 8.2 The test piece shall be firmly supported such that there is no significant change in the testing machine compliance. The test piece shall either be placed on a support that is rigid in the direction of indentation or be fixed in a suitable test piece holder. The contact surfaces between test piece support and test piece holder shall be free from extraneous matter, which can increase the compliance (reduce the stiffness) of the test piece support.
If the sample is supported by materials or mounting methods other than those used when determining the machine compliance, then the different elastic response of these materials and mounting methods can cause additional compliance. A certified reference material, mounted in the same way as the sample, should be
...